Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Zytel® ST801AW NC010 Nylon 66  (Unverified Data**)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: Zytel® ST801AW NC010 is a Super Tough, high performance polyamide 66 resin. It is UV stabilized and when appropriately colored offers the best resistance to indirect sunlight in automotive interior applications.

This product line has been acquired from DuPont by Celanese. This specific page is outdated and not maintained. If the product is active, it can be found under its current Celanese listing.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.08 g/ccDAM; ISO 1183
Water Absorption 1.17 %
@Temperature 23.0 °C
DAM; Immersion 24h; ISO 62, Similar to
Moisture Absorption at Equilibrium 1.9 %
@Thickness 1.00 mm,
Temperature 23.0 °C
50% RH; from DAM; ISO 62, Similar to
Linear Mold Shrinkage, Flow 0.020 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.018 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 110DAM; ISO 2039/2
Tensile Strength at Break 45.0 MPa
@Temperature 23.0 °C
DAM; 50mm/min; ISO 527
 48.0 MPa
@Temperature 23.0 °C
50%RH; 50mm/min; ISO 527
Tensile Strength, Yield 35.5 MPa
@Temperature 23.0 °C
50%RH; ISO 527
 49.0 MPa
@Temperature 23.0 °C
DAM; ISO 527
Tensile Stress at Strain 48.0 MPa
@Strain 50 %,
Temperature 23.0 °C
50%RH; ISO 527
 50.0 MPa
@Strain 50 %,
Temperature 23.0 °C
DAM; ISO 527
Elongation at Break 44 %
@Temperature 23.0 °C
DAM; ISO 527
 >= 50 %
@Temperature 23.0 °C
50%RH; ISO 527
 >= 50 %
@Temperature 23.0 °C
DAM; ISO 527
 >= 50 %
@Temperature 23.0 °C
50%RH; ISO 527
 74 %
@Temperature 23.0 °C
DAM; 50mm/min; ISO 527
Elongation at Yield 5.0 %
@Temperature 23.0 °C
DAM; ISO 527
 26.5 %
@Temperature 23.0 °C
50%RH; ISO 527
Tensile Modulus 775 MPa
@Temperature 23.0 °C
50%RH; ISO 527
 1900 MPa
@Temperature 23.0 °C
DAM; ISO 527
Flexural Modulus 728 MPa
@Temperature 23.0 °C
50%RH; ISO 178
 1800 MPa
@Temperature 23.0 °C
DAM; ISO 178
Izod Impact, Notched (ISO) 21.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 180/1A
 77.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
Izod Impact, Unnotched (ISO) NB
@Temperature -30.0 °C
DAM; ISO 180/1U
 NB
@Temperature 23.0 °C
DAM; ISO 180/1U
Charpy Impact Unnotched 240 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eU
 260 kJ/m²
@Temperature 0.000 °C
DAM; ISO 179/1eU
 300 kJ/m²
@Temperature -20.0 °C
DAM; ISO 179/1eU
 NB
@Temperature -30.0 °C
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 21.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eA
 22.0 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eA
 22.0 kJ/m²
@Temperature -20.0 °C
DAM; ISO 179/1eA
 23.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 36.0 kJ/m²
@Temperature 0.000 °C
DAM; ISO 179/1eA
 83.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 2.40e+12 ohm-cm
@Temperature 23.0 °C
50%RH; IEC 60093
 2.50e+16 ohm-cm
@Temperature 23.0 °C
DAM; IEC 60093
Surface Resistance 7.10e+12 ohm
@Temperature 23.0 °C
50%RH; IEC 60093
 2.70e+15 ohm
@Temperature 23.0 °C
DAM; IEC 60093
Dielectric Constant 3.2
@Frequency 1e+6 Hz,
Temperature 23.0 °C
DAM; IEC 60250
 3.4
@Frequency 100 Hz,
Temperature 23.0 °C
DAM; IEC 60250
 3.5
@Frequency 1e+6 Hz,
Temperature 23.0 °C
50%RH; IEC 60250
 6.0
@Frequency 100 Hz,
Temperature 23.0 °C
50%RH; IEC 60250
Dielectric Strength 26.0 kV/mm
@Thickness 2.00 mm,
Temperature 23.0 °C
50%RH; IEC 60243-1
 26.0 kV/mm
@Thickness 2.00 mm,
Temperature 23.0 °C
DAM; IEC 60243-1
Dissipation Factor 0.0050
@Frequency 100 Hz,
Temperature 23.0 °C
DAM; IEC 60250
 0.011
@Frequency 1e+6 Hz,
Temperature 23.0 °C
DAM; IEC 60250
 0.038
@Frequency 1e+6 Hz,
Temperature 23.0 °C
50%RH; IEC 60250
 0.176
@Frequency 100 Hz,
Temperature 23.0 °C
50%RH; IEC 60250
Comparative Tracking Index 600 V
@Thickness 3.00 mm,
Temperature 23.0 °C
DAM; UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 120 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ASTM E 831
 120 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 130 µm/m-°C
@Temperature -30.0 - 30.0 °C
DAM; ISO 11359-1/-2
 130 µm/m-°C
@Temperature -30.0 - 30.0 °C
DAM; ASTM E 831
 140 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ASTM E 831
 140 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ISO 11359-1/-2
 170 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ASTM E 831
 170 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°C
@Temperature -30.0 - 30.0 °C
DAM; ISO 11359-1/-2
 110 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 110 µm/m-°C
@Temperature -30.0 - 30.0 °C
DAM; ASTM E 831
 110 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ASTM E 831
 120 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ASTM E 831
 120 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ISO 11359-1/-2
 120 µm/m-°C
@Temperature 55.0 - 160 °C
DAM; ISO 11359-1/-2
 120 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ASTM E 831
Melting Point 262 °CDAM; 10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 155 °CDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °CDAM; ISO 75-1/-2
UL RTI, Electrical 125 °C
@Thickness 0.750 mm
DAM; UL 746B
UL RTI, Mechanical with Impact 75.0 °C
@Thickness 0.750 mm
DAM; UL 746B
UL RTI, Mechanical without Impact 85.0 °C
@Thickness 0.750 mm
DAM; UL 746B
Flammability, UL94 HB
@Thickness 0.750 mm
DAM; IEC 60695-11-10
 HB
@Thickness 0.750 mm
DAM; UL94
 
Processing PropertiesOriginal ValueComments
Melt Temperature 270 - 300 °CDAM
 290 °CDAM; optimum
Mold Temperature 70.0 °CDAM; Optimum
 50.0 - 90.0 °CDAM
Drying Temperature 80.0 °CDAM
Dry Time 2.00 - 4.00 hourDAM; Dehumidified Dryer
Moisture Content <= 0.20 %DAM
 
Descriptive Properties
AdditiveImpact Modifier
 UV Stabilizer
AppearanceNatural Color
Drying RecommendedYes, if moisture content of resin exceeds recommended level
FeaturesChemical Resistance, Good
 Fuel Resistant
 Grease Resistant
 Impact Modified
 Impact Resistance, High
 Oil Resistant
 Toughness, Low Temperature
 Toughness, Ultra High
FormsPellets
GenericNylon 66
Material StatusCurrent
Part Marking Code>PA66-HI<ISO 11469
Polymer FamilyPolyamide
Polymer TypePA66
Processing MethodInjection Molding
Product CategoryToughened Resins
 Unreinforced Resins
 UV Resistant/Weatherable Resins
Region Available - GlobalYes
Resin IdentificationPA66-HIISO 1043
Ultrasonic WeldableYes
UsesAppliance Components
 Automotive Applications
 Electrical/Electronic Applications
 Industrial Applications
 Sporting Goods

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® A3Z HP PA66 (Dry)
BASF Ultramid® A3L HP UV BK 23220 PA66 (Dry)
LyondellBasell Sequel 1823-UV 7C45 Thermoplastic Olefinic Elastomer
Celanese Zytel® ST801AW NC010 PA66-HI
Celanese Zytel® ST801AW BK195 PA66-HI

PDSZ1508 / 142602

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.