MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
LyondellBasell Petrothene® NA942000 Low Density Polyethylene, Film Extrusion Grade  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Film Grade

Material Notes: PETROTHENE NA942 is a series of resins designed especially for heavy duty film applications, such as bags used to package fertilizer, peat moss, decorative stone and agricultural and construction materials. NA942 exhibits excellent impact properties and puncture resistance.

Regulatory Status: The basic resin NA942 meets the requirements of the Food and Drug Administration regulation, 21 CFR 177.1520. This regulation allows the use of this olefin polymer in "...articles or components of articles intended for use in contact with food." Specific limitations or conditions of use may apply. Contact your Equistar sales representative for further information regarding the suitability of specific products for specific applications.

Generally recommended extrusion conditions include a melt temperature range of 330°-430°F (165°- 221°C); a blow-up ratio range of 1.8-2.5:1. Drawdown to 2.0 mils (51 microns) is possible at commercial rates when proper extrusion techniques are used.

This product is from the former Equistar product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.920 g/ccASTM D1505
ESCR 100% Igepal® 168 hourno failures; molding; ASTM D1693
Thickness 2.00 mil
Melt Flow 0.18 g/10 minASTM D1238
Antiblock Level 0.000 ppm
Slip Level 0.000 ppm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 42molding; ASTM D2240
Tensile Strength at Break 2600 psimolding; ASTM D638
Tensile Strength, Yield 1400 psimolding; ASTM D638
Film Elongation at Break, MD 300 %ASTM D882
Film Elongation at Break, TD 450 %ASTM D882
Elongation at Break 750 %molding; ASTM D638
Elongation at Yield 100 %molding; ASTM D638
Dart Drop 110 g/milF50; ASTM D1709
Film Tensile Strength at Break, MD 3000 psiASTM D882
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature <= -75.0 °CF50; molding; ASTM D746
 
Processing PropertiesOriginal ValueComments
Melt Temperature 430 °F
Die Opening 0.0635 cm
Blow-up Ratio (BUR) 2.0
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PEQU0847 / 104203

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.