MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
AISI 1021 Steel, normalized at 925°C (1700°F), air cooled, 50 mm (2 in.) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Low Carbon Steel

Material Notes: Used in cold heading and extruding. Applications include low-strength fasteners, die pins, motor spindles, and recessed-head screws. Post water quenched hardness: 38 HRC surface, 88 HRB half-radius, 84 HRB center.

Key Words: UNS G10210, ASTM A29, ASTM A510, ASTM A519, ASTM A545, ASTM A548, ASTM A576, carbon steels, ASTM A659, SAE J403, SAE J412, SAE J414, BS 970 070M20, EN3, BS 970 080M20
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.858 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 137
Hardness, Knoop 156Converted from Brinell
Hardness, Rockwell B 75Converted from Brinell
Hardness, Vickers 143Converted from Brinell
Tensile Strength, Ultimate 474 MPa
Tensile Strength, Yield 330 MPa
Elongation at Break 34 %in 50 mm
Reduction of Area 66.6 %
Modulus of Elasticity 200 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steel
Poissons Ratio 0.29Typical For Steel
Shear Modulus 80.0 GPaTypical for steel
Izod Impact 118 J
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000159 ohm-cm
@Temperature 0.000 °C
estimated by comparison with similar steel alloys
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.5 µm/m-°C
@Temperature 20.0 °C
Typical steel
 12.2 µm/m-°C
@Temperature 0.000 - 300 °C
Typical for steel
 13.9 µm/m-°C
@Temperature 0.000 - 500 °C
Typical for steel
Specific Heat Capacity 0.472 J/g-°CTypical steel
Thermal Conductivity 51.9 W/m-KTypical steel
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.17 - 0.23 %
Iron, Fe 98.78 - 99.23 %As remainder
Manganese, Mn 0.60 - 0.90 %
Phosphorus, P <= 0.040 %
Sulfur, S <= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1021 Steel, normalized at 925°C (1700°F), air cooled, 100 mm (4 in.) round
AISI 1021 Steel, cold drawn
AISI 1021 Steel, mock carburized at 910°C (1670°F) for 8 hours, 775°C (1430°F) reheat, water quenched, 175°C (350°F) temper, 13 mm (0.5 in.) round
AISI 1021 Steel, normalized at 925°C (1700°F), air cooled, 25 mm (1 in.) round
AISI 1021 Steel, normalized at 925°C (1700°F), air cooled, 13 mm (0.5 in.) round

M1021G / 6846

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.