MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Rogers Arlon 28561R015 0.015" (0.381 mm) Uncured Silicone Rubber with Fiberglass Substrate
Categories: Polymer; Thermoset; Silicone; Silicone Rubber; Silicone, Molded, Glass Fiber Filled

Material Notes: Design/Construction:
Interleave 1: Polyethylene
Side 1: Uncured Silicone Rubber
Substrate: Style 1528 Fiberglass
Side 2: Uncured Silicone Rubber
Interleave 2: Polyethylene

Appearance: Red silicone gum on fiberglass fabric

This data represents typical values for the production material. The data should not be used to write, or in place of, material specifications.

Information provided by Arlon Silicone Technologies Division; now a part of Rogers Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.21 g/cc0.0437 lb/in³Silicone Property; Arlon SQA-TMS-024
Thickness 38.1 microns1.50 milInterleave 1
 38.1 microns1.50 milInterleave 2
 88.9 microns3.50 milSide 1; Arlon SQA-TMS-003
 88.9 microns3.50 milSide 2; Arlon SQA-TMS-003
 203 microns8.00 milS
 381 microns15.0 milOverall; Arlon SQA-TMS-003
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 3939Silicone Property; ASTM D2240
Tensile Strength 5.93 MPa860 psiSilicone Property; ASTM D412
Elongation at Break 720 %720 %Silicone Property; ASTM D412
Tear Strength 20.2 kN/m115 pliSilicone Property; ASTM D624
Peel Strength 1.30 kN/m7.40 pliBond Strength; Arlon SQA-TMS-029
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 27.6 kV/mm700 kV/inASTM D149
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 232 °C450 °F
Minimum Service Temperature, Air -56.7 °C-70.0 °F
 
Processing PropertiesMetricEnglishComments
Cure Time 120 min
@Temperature 204 °C
2.00 hour
@Temperature 400 °F
Recommended Postcure Cycle
 15.0 min
@Pressure 0.345 MPa,
Temperature 177 °C
0.250 hour
@Pressure 50.0 psi,
Temperature 350 °F
Recommended Cure Cycle
Shelf Life 6.00 Month
@Temperature 23.9 °C
6.00 Month
@Temperature 75.0 °F
From date of manufacture
 
Descriptive Properties
ColorRed
Total Product Weight (oz/yd2)16.2Arlon SQA-TMS-025

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Rogers Arlon 28540R015 0.016" (0.406 mm) Uncured Silicone Rubber with Fiberglass Substrate
Dow C6-350LH ELASTOMER KIT
Dow C6-180 ELASTOMER KIT
Dow 5-8601 FLUOROSILICONE LSR, KIT
Dow 3-6891 1-PART SILICONE RUBBER ABRADABLE SEALANT COMPOUND

PARL134 / 125320

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.