MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Rogers Arlon Thermabond® 48A43X008 0.008"(0.203 mm) Cured Silicone Rubber with Fiberglass Substrate
Categories: Polymer; Thermoset; Silicone; Silicone Rubber; Silicone, Molded, Glass Fiber Filled

Material Notes: Description: Thermabond® Electrically insulating, thermally conductive, thermal interface material (TIM).

Design/Construction:
Side 1: Cured Silicone Rubber
Substrate: Style 1080 Fiberglass
Side 2: Cured Silicone Rubber
Liner: Polyethylene

This data represents typical values for the production material. The data should not be used to write, or in place of, material specifications.

Information provided by Arlon Silicone Technologies Division; now a part of Rogers Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.80 g/cc0.101 lb/in³Silicone Property; Arlon SQA-TMS-024
Thickness 63.5 microns2.50 milSide 1; Arlon SQA-TMS-003
 63.5 microns2.50 milSide 2; Arlon SQA-TMS-003
 76.2 microns3.00 milSubstrate; Arlon SQA-TMS-003
 203 microns8.00 milOverall; Arlon SQA-TMS-003
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7777Silicone Property; ASTM D2240
Tensile Strength 4.72 MPa685 psiSilicone Property; ASTM D412
Tensile Strength, Yield 24.5 MPa
@Strain <=1 %
3550 psi
@Strain <=1 %
Silicone Property; Arlon SQA-TMS-008
Elongation at Break 120 %120 %Silicone Property; ASTM D412
Poissons Ratio 0.500.50Approximately, Silicone Property
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 6.91
@Frequency 1e+6 Hz
6.91
@Frequency 1e+6 Hz
Silicon Property; IPC TM 650 - 2.5.5.3
Dielectric Strength 25.2 kV/mm640 kV/inASTM D149
Dissipation Factor 0.0044
@Frequency 1e+6 Hz
0.0044
@Frequency 1e+6 Hz
Silicon Property; IPC TM 650 - 2.5.5.3
 
Thermal PropertiesMetricEnglishComments
CTE, linear 150 µm/m-°C
@Temperature 20.0 - 160 °C
83.3 µin/in-°F
@Temperature 68.0 - 320 °F
Silicone Property; ASTM E 831
Specific Heat Capacity 0.820 J/g-°C
@Temperature 100 °C
0.196 BTU/lb-°F
@Temperature 212 °F
Silicone Property; Arlon SQA-TMS-052
Thermal Conductivity 1.40 W/m-K
@Temperature 100 °C
9.72 BTU-in/hr-ft²-°F
@Temperature 212 °F
Silicone Property; ASTM E 1530
 1.70 W/m-K
@Pressure 30.0 MPa,
Temperature 50.0 °C
11.8 BTU-in/hr-ft²-°F
@Pressure 4350 psi,
Temperature 122 °F
Product Property; Arlon SQA-TMS-054
Maximum Service Temperature, Air 95.6 °C204 °F
Minimum Service Temperature, Air -73.3 °C-100 °F
Glass Transition Temp, Tg 118 °C244 °FSilicone Property; ASTM D3418
 
Processing PropertiesMetricEnglishComments
Shelf Life 60.0 Month
@Temperature 21.0 - 27.0 °C
60.0 Month
@Temperature 69.8 - 80.6 °F
From date of manufacture
 
Descriptive Properties
ColorGray
 Naturally WhiteSubstrate
Plasticity2.3 mmArlon-SQA-TMS-005
Total Product Weight (g/m2)432Arlon SQA-TMS-025

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PARL244 / 125430

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.