MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Idemitsu Kosan TARFLON™ 2200 Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: Standard A220. Superior mold release IR200 (ice color). Weather resistance, superior mold release IV200R (ice color).

Polycarbonate is known for its high impact resistance, good transparency and heat resistance, and superb precision and electrical properties. TARFLON is used in a wide range of applications such as house wares, office equipment , mobile devices, communication equipment ,display device such as LCD backlight parts, automotive ,lighting and many fields.

Information provided by Idemitsu Losan Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ISO 1183(JIS K7112)
Moisture Absorption 0.230 %
@Time 86400 sec
0.230 %
@Time 24.0 hour
50% RH; ISO 62(JIS K7209)
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 2.00 mm
0.0050 - 0.0070 in/in
@Thickness 0.0787 in
Idemitsu Method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
@Thickness 2.00 mm
0.0050 - 0.0070 in/in
@Thickness 0.0787 in
Idemitsu Method
Melt Flow 14.4 g/10 min
@Load 1.20 kg,
Temperature 300 °C
14.4 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ISO 1133 (JIS K7210)
Spiral Flow 16.0 cm
@Thickness 2.00 mm
6.30 in
@Thickness 0.0787 in
Width:10mm. Cylinder: 240°C/Mold: 40°C. Inj.Pressure: 125 MPa.; Idemitsu Method
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 5050ISO 2039-2 (JIS K7202-2)
Hardness, Rockwell R 120120ISO 2039-2 (JIS K7202-2)
Tensile Strength, Yield 65.0 MPa9430 psiISO 527-1,2 (JIS K7161, 7162)
Elongation at Break 95 %95 %Nominal; ISO 527-1,2 (JIS K7161, 7162)
Flexural Strength 90.0 MPa13100 psiISO 178 (JIS K7171)
Flexural Modulus 2.30 GPa334 ksiISO 178 (JIS K7171)
Charpy Impact, Notched 8.00 J/cm²38.1 ft-lb/in²ISO 179-1(JIS K7111)
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cmASTM D257
Dielectric Constant  2.85
@Frequency 1e+6 Hz
2.85
@Frequency 1e+6 Hz
IEC 60250
 2.91
@Frequency 100 Hz
2.91
@Frequency 100 Hz
IEC 60250
Dielectric Strength 30.0 kV/mm762 kV/inIEC 60243-1(JIS C2110)
Dissipation Factor  0.00066
@Frequency 100 Hz
0.00066
@Frequency 100 Hz
IEC 60250
 0.0092
@Frequency 1e+6 Hz
0.0092
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 60 - 120 sec60 - 120 secASTM D495
Comparative Tracking Index 250 - 400 V250 - 400 VUL746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear 65.0 µm/m-°C36.1 µin/in-°FISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 125 °C257 °FISO 75-1,2(JIS K7191-1,2)
UL RTI, Electrical 130 °C
@Thickness 0.360 mm
266 °F
@Thickness 0.0142 in
UL746B
UL RTI, Mechanical with Impact 125 °C
@Thickness 0.360 mm
257 °F
@Thickness 0.0142 in
UL746B
UL RTI, Mechanical without Impact 130 °C
@Thickness 0.360 mm
266 °F
@Thickness 0.0142 in
UL746B
Flammability, UL94 V-2
@Thickness 0.360 - 1.80 mm
V-2
@Thickness 0.0142 - 0.0709 in
 
Optical PropertiesMetricEnglishComments
Transmission, Visible 85 - 89 %85 - 89 %Total Luminous; ISO 13468-1 (JIS K7361-1)
 
Processing PropertiesMetricEnglishComments
Melt Temperature 260 - 300 °C500 - 572 °FCylinder Temperature
 <= 320 °C<= 608 °FMax Cylinder Temperature
Mold Temperature 80.0 - 120 °C176 - 248 °F
Drying Temperature 120 °C
@Time 18000 - 28800 sec
248 °F
@Time 5.00 - 8.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PIDEM203 / 249567

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.