MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ THERMOTUF™ PF006I Nylon 6 (Americas)  (Unverified Data**)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled

Material Notes: LNP THERMOTUF* PF006I is a compound based on Nylon 6 resin containing 30% Glass Fiber. Added features of this material include: High Impact.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.35 g/cc1.35 g/ccASTM D792
Density 1.35 g/cc0.0488 lb/in³ASTM D792
 1.37 g/cc0.0495 lb/in³ISO 1183
Moisture Absorption 0.830 %0.830 %23°C / 50% RH; ISO 62
 0.830 %0.830 %50% RH, 24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.0010 - 0.0030 cm/cm0.0010 - 0.0030 in/in24 hrs; ASTM D955
 0.0011 - 0.0030 cm/cm0.0011 - 0.0030 in/in24 hrs; ISO 294
Linear Mold Shrinkage, Transverse 0.0062 - 0.0067 cm/cm0.0062 - 0.0067 in/in24 hrs; ISO 294
 0.0090 - 0.020 cm/cm0.0090 - 0.020 in/in24 hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 97.0 MPa14100 psiType I, 5 mm/min; ASTM D638
 99.0 MPa14400 psi5 mm/min; ISO 527
Tensile Strength, Yield 35.0 MPa5080 psi5 mm/min; ISO 527
 50.0 MPa7250 psiType I, 5 mm/min; ASTM D638
Elongation at Break 8.1 %8.1 %Type I, 5 mm/min; ASTM D638
Flexural Strength 157 MPa22800 psi1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 6.82 GPa989 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 1.06 J/cm1.99 ft-lb/inASTM D256
Izod Impact, Unnotched 7.27 J/cm13.6 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 10.0 kJ/m²4.76 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 53.0 kJ/m²25.2 ft-lb/in²80*10*4; ISO 180/1U
Impact Test 4.00 J2.95 ft-lbMultiaxial Impact; ISO 6603
Instrumented Impact Energy at Peak 16.0 J11.8 ft-lbASTM D3763
Tangent Modulus 9650 MPa1.40e+6 psi1 mm/min; ISO 527
 16230 MPa2.354e+6 psi50 mm/min; ASTM D638
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 141 °C286 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 139 °C
@Thickness 3.20 mm
282 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 135 °C275 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 137 °C
@Thickness 3.20 mm
279 °F
@Thickness 0.126 in
unannealed; ASTM D648
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
UL 94 by SABIC-IP
 
Processing PropertiesMetricEnglishComments
Zone 1 250 - 260 °C482 - 500 °F
Zone 2 265 - 275 °C509 - 527 °F
Zone 3 275 - 290 °C527 - 554 °F
Melt Temperature 265 - 275 °C509 - 527 °F
Mold Temperature 80.0 - 95.0 °C176 - 203 °F
Drying Temperature 80.0 °C176 °F
Dry Time 4.00 hour4.00 hour
Moisture Content 0.15 - 0.25 %0.15 - 0.25 %
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI21018 / 214154

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.