MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
NOVA Chemicals Sclair® 11J1 Octene LLDPE Film Resin  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade; LLDPE/Octene, Film

Material Notes: Film Properties. Features: Low gel, excellent hermetic heat sealability, easy processability, high toughness and strength.

Applications: Sealant web in food packaging, vacuum packaging, barrier applications, etc.

Data provided by the manufacturer.

Key Words: Linear Low Density Polyethylene; Polyoctene; Polyolefin
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.920 g/ccASTM D792
Melt Flow 0.95 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 9.00 MPaASTM D882
Film Tensile Strength at Yield, TD 10.0 MPaASTM D882
Film Elongation at Break, MD 675 %ASTM D882
Film Elongation at Break, TD 880 %ASTM D882
Secant Modulus, MD 0.176 GPaASTM D882
Secant Modulus, TD 0.200 GPaASTM D882
Coefficient of Friction 0.80ASTM D1894
Elmendorf Tear Strength, MD 18.0 g/micronASTM D1922
Elmendorf Tear Strength, TD 24.0 g/micronASTM D1922
Dart Drop 7.00 g/micronF 50; ASTM D1709/A
Film Tensile Strength at Break, MD 41.0 MPaASTM D882
Film Tensile Strength at Break, TD 33.0 MPaASTM D882
 
Optical PropertiesOriginal ValueComments
Haze 10 %
@Thickness 0.0250 mm
ASTM D1003
Gloss 58 %45°; 1 mil; ASTM D1894
 
Processing PropertiesOriginal ValueComments
Melt Temperature 220 - 230 °C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
NOVA Chemicals Sclair® FP120-D Octene LLDPE Film Resin
NOVA Chemicals Sclair® 11J4 Octene LLDPE Film Resin
NOVA Chemicals Surpass® FPs117-C Octene Copolymer sLLDPE Film Resins
NOVA Chemicals Sclair® FP026-F Octene LLDPE Film Resin
NOVA Chemicals Sclair® FPr017-D Octene LLDPE Film Resin

PEHN06 / 35519

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.