MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Ovako 11SMn30, Green Cut 2715 Steel, +SH
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: Green Cut steel has been developed to replace leaded free-cutting steels, when the customer is looking for an environmentally friendly alternative. High sulfur content combined with M-treatment gives superior machinability both with carbide and HSS tools.

M-SteelThe concept: Our M-Steel treatment can be applied to any steel grade. The basis for the concept is that non-metallic inclusions are modified and controlled with calcium treatment. These inclusions are modified in a way to maximize machinability and to improve transverse fatigue strength. In this way, a protective layer is formed on the cutting tool during machining that very significantly reduces the wear on the tool and increases the tool life. At every stage of the M-Steel production process the material is optimised to improve machinability, from raw material through melt, to casting, hot rolling and the final heat treatment. Individual delivery requirements can be met to supply your material in the best form for your machines in compliance with tight straightness and dimensional tolerances. M-Steel has a consistent machinability from cast to cast, meaning that machines can be run with fixed high cutting rates and predictable tool change intervals from one production run to another. Recent findings also show that the MSteel effect is particularly pronounced in turning in very hard condition using Cubic Boron Nitride (CBN) inserts. Replacing traditional grinding of case- or induction-hardened surfaces with Hard Part Turning can mean very large cost savings, together with production lead time and quality improvements.

Information provided by Ovako

Key Words: SS 1912, SS 1914
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 120 - 160
@Thickness 23.0 - 125 mm
Tensile Strength 360 - 540 MPa
@Thickness 23.0 - 125 mm
Tensile Strength, Yield >= 270 MPa
@Thickness 23.0 - 125 mm
Elongation at Break 22 %
@Thickness 23.0 - 125 mm
Modulus of Elasticity 210 GPa
Poissons Ratio 0.30
Shear Modulus 80.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
Thermal Conductivity 40.0 - 45.0 W/m-KAmbient temperature
Transformation Temperature 436 °CMS
 715 °CAC1
 843 °CAC3
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.050 - 0.14 %
Iron, Fe 97.68 - 98.68 %As Balance
Manganese, Mn 1.0 - 1.4 %
Phosphorus, P <= 0.050 %
Silicon, Si 0.050 - 0.40 %
Sulfur, S 0.22 - 0.33 %
 
Descriptive Properties
WeldabilityCEV 0.4max
 Pcm 0.22max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ovako 11SMn30, Green Cut 2715 Steel, +C
Ovako 11SMn30, Green Cut 2715 Steel, +AR
AISI Type A2 Tool Steel
AISI 1215 Steel, cold drawn, 19-38 mm round
AISI 1010 Steel, hot rolled bar, 19-32 mm (0.75-1.25 in) round or thickness

NOVAKO064 / 234363

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.