MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
SABIC VALOX™ 735 PBT (Europe)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: 40% glass/mineral, excellent thermal performance/low shrink. Motorized heating appliances, adaptor rings, oven grills, etc. Black/natural only.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.62 g/ccASTM D792
Density 1.62 g/ccISO 1183
Filler Content 40 %ASTM D229
Water Absorption 0.96 %23°C/sat; ISO 62
Moisture Absorption 0.0700 %23°C / 50% RH; ISO 62
Viscosity 160 cP
@Shear Rate 1500 1/s,
Temperature 260 °C
melt; ISO 11443
Linear Mold Shrinkage, Flow 0.0030 - 0.0060 cm/cmSABIC method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0080 cm/cmSABIC method
Melt Flow 1.0 g/10 min
@Load 5.00 kg,
Temperature 250 °C
cm³/10 min; ISO 1133
 3.0 g/10 min
@Load 1.20 kg,
Temperature 265 °C
cm³/10 min; ISO 1133
 15 g/10 min
@Load 5.00 kg,
Temperature 265 °C
cm³/10 min; ISO 1133
 20 g/10 min
@Load 5.00 kg,
Temperature 266 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 124ISO 2039-2
Ball Indentation Hardness 144 MPaISO 2039-1
Tensile Strength at Break 90.0 MPa5 mm/min; ISO 527
 95.0 MPa5 mm/min; ASTM D638
Tensile Strength, Yield 90.0 MPa5 mm/min; ISO 527
 95.0 MPa5 mm/min; ASTM D638
Elongation at Break 2.0 %5 mm/min; ASTM D638
 2.0 %5 mm/min; ISO 527
Elongation at Yield 2.0 %5 mm/min; ISO 527
 2.0 %5 mm/min; ASTM D638
Tensile Modulus 10000 MPa1mm/min; ISO 527
 10400 MPa5 mm/min; ASTM D638
Flexural Strength 124 MPabrk, 1.3 mm/min, 50 mm span; ASTM D790
 130 MPa2 mm/min; break; ISO 178
Flexural Yield Strength 120 MPa1.3 mm/min, 50 mm span; ASTM D790
 130 MPa2 mm/min; ISO 178
Flexural Modulus 8300 MPa1.3 mm/min, 50 mm span; ASTM D790
 8300 MPa2 mm/min; ISO 178
Flexural Strain at Break 2.0 %2 mm/min; ISO 178
Izod Impact, Notched 60.0 J/mASTM D256
 50.0 J/m
@Temperature -30.0 °C
ASTM D256
 55.0 J/m
@Temperature 0.000 °C
ASTM D256
Izod Impact, Unnotched 560 J/mASTM D4812
 520 J/m
@Temperature -30.0 °C
ASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature 0.000 °C
80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 35.0 kJ/m²80*10*4; ISO 180/1U
 25.0 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched 35.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eU
 40.0 kJ/m²ISO 179/2C
 30.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
 30.0 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
Charpy Impact, Notched 4.00 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 7.00 kJ/m²ISO 179/2C
 4.00 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
 7.00 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
Taber Abrasion, mg/1000 Cycles 64CS-17, 1 kg; SABIC method
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmASTM D257
 >= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant 3.3
@Frequency 1e+6 Hz
IEC 60250
 3.5
@Frequency 50.0 - 60.0 Hz
IEC 60250
Dielectric Strength 18.0 kV/mm
@Thickness 3.20 mm
in oil; ASTM D149
 18.0 kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
 22.0 kV/mm
@Thickness 1.60 mm
in oil; IEC 60243-1
 22.0 kV/mm
@Thickness 1.60 mm
in oil; ASTM D149
 45.0 kV/mm
@Thickness 0.800 mm
in oil; ASTM D149
 45.0 kV/mm
@Thickness 0.800 mm
in oil; IEC 60243-1
Dissipation Factor 0.0080
@Frequency 50.0 - 60.0 Hz
IEC 60250
 0.017
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 60 - 120 secASTM D495
Comparative Tracking Index 250 - 400 VUL 746A
Hot Wire Ignition, HWI >= 120 secUL 746A
High Amp Arc Ignition, HAI 15 - 30 arcsUL 746A
High Voltage Arc-Tracking Rate, HVTR 10.0 - 25.4 mm/minUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 21.8 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
 22.8 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 25.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 65.3 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 80.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 140 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
Thermal Conductivity 0.360 W/m-KISO 8302
Hot Ball Pressure Test 125 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 215 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 215 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 190 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 190 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 180 °CRate B/120; ISO 306
 180 °CRate B/50; ISO 306
 185 °CRate B/50; ASTM D1525
 220 °CRate A/50; ISO 306
 220 °CRate A/50; ASTM D1525
UL RTI, Electrical 140 °CUL 746B
UL RTI, Mechanical with Impact 140 °CUL 746B
UL RTI, Mechanical without Impact 140 °CUL 746B
Flammability, UL94 HB
@Thickness 3.00 mm
UL 94
 HB
@Thickness 0.810 mm
UL 94
Glow Wire Test 750 °C
@Thickness 1.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Processing Temperature 40.0 - 60.0 °CHopper Temperature
Nozzle Temperature 265 - 275 °CInjection Molding
Zone 1 240 - 260 °C
Zone 2 255 - 280 °C
Zone 3 260 - 280 °C
Melt Temperature 260 - 285 °C
Mold Temperature 60.0 - 110 °C
Drying Temperature 110 - 120 °CInjection Molding
Dry Time 4.00 - 6.00 hourInjection Molding
Moisture Content 0.020 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10237 / 243704

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.