Physical Properties | Original Value | Comments |
---|
Density | 1.65 g/cc |
Moisture Absorption | 1.50 % |
Linear Mold Shrinkage, Flow | 0.0035 cm/cm |
Linear Mold Shrinkage, Transverse | 0.0090 cm/cm |
|
Mechanical Properties | Original Value | Comments |
---|
Tensile Strength at Break | 82.0 MPa @Temperature 200 °C |
| 90.0 MPa @Temperature 180 °C |
| 105 MPa @Temperature 120 °C |
| 105 MPa @Temperature 160 °C |
| 115 MPa @Temperature 100 °C |
| 115 MPa @Temperature 150 °C |
| 140 MPa @Temperature 80.0 °C |
| 155 MPa @Temperature 120 °C |
| 195 MPa @Temperature 100 °C |
| 220 MPa @Temperature 40.0 °C |
| 220 MPa @Temperature 80.0 °C |
| 240 MPa @Temperature 23.0 °C |
| 250 MPa @Temperature 40.0 °C |
| 260 MPa @Temperature 23.0 °C |
| 280 MPa @Temperature -40.0 °C |
| 290 MPa @Temperature -40.0 °C |
Elongation at Break | 2.0 % @Temperature 23.0 °C |
| 2.0 % @Temperature -40.0 °C |
| 2.0 % @Temperature -40.0 °C |
| 2.1 % @Temperature 23.0 °C |
| 2.1 % @Temperature 40.0 °C |
| 2.1 % @Temperature 40.0 °C |
| 2.3 % @Temperature 80.0 °C |
| 2.6 % @Temperature 100 °C |
| 3.6 % @Temperature 120 °C |
| 4.0 % @Temperature 80.0 °C |
| 4.5 % @Temperature 100 °C |
| 5.5 % @Temperature 120 °C |
| 5.7 % @Temperature 150 °C |
| 6.0 % @Temperature 160 °C |
| 6.0 % @Temperature 180 °C |
| 6.0 % @Temperature 200 °C |
Tensile Modulus | 6800 MPa @Temperature 200 °C |
| 7100 MPa @Temperature 180 °C |
| 7700 MPa @Temperature 120 °C |
| 7700 MPa @Temperature 160 °C |
| 8200 MPa @Temperature 150 °C |
| 8700 MPa @Temperature 100 °C |
| 10900 MPa @Temperature 80.0 °C |
| 12400 MPa @Temperature 120 °C |
| 15700 MPa @Temperature 100 °C |
| 16800 MPa @Temperature 80.0 °C |
| 17200 MPa @Temperature 40.0 °C |
| 17600 MPa @Temperature 40.0 °C |
| 18000 MPa @Temperature 23.0 °C |
| 18300 MPa @Temperature 23.0 °C |
| 18300 MPa @Temperature -40.0 °C |
| 18500 MPa @Temperature -40.0 °C |
Flexural Strength | 310 MPa |
| 390 MPa |
Flexural Modulus | 6000 MPa @Temperature 200 °C |
| 6400 MPa @Temperature 180 °C |
| 7500 MPa @Temperature 160 °C |
| 11700 MPa @Temperature 120 °C |
| 17300 MPa @Temperature 23.0 °C |
| 17800 MPa @Temperature 23.0 °C |
Fatigue Strength | 100 MPa @# of Cycles 316 |
Charpy Impact Unnotched | 65.0 kJ/m² @Temperature -30.0 °C |
| 75.0 kJ/m² @Temperature -30.0 °C |
| 80.0 kJ/m² @Temperature 23.0 °C |
| 90.0 kJ/m² @Temperature 23.0 °C |
Charpy Impact, Notched | 9.00 kJ/m² @Temperature -30.0 °C |
| 10.0 kJ/m² @Temperature 23.0 °C |
| 11.0 kJ/m² @Temperature -30.0 °C |
| 12.0 kJ/m² @Temperature 23.0 °C |
|
Electrical Properties | Original Value | Comments |
---|
Volume Resistivity | >= 1.00e+13 ohm-cm |
| >= 1.00e+13 ohm-cm |
Dielectric Constant | 4.8 @Frequency 1e+6 Hz |
| 5.0 @Frequency 1e+6 Hz |
| 5.1 @Frequency 100 Hz |
| 5.8 @Frequency 100 Hz |
Comparative Tracking Index | 425 V |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 30.0 µm/m-°C |
CTE, linear, Parallel to Flow | 27.0 µm/m-°C |
Melting Point | 325 °C |
Maximum Service Temperature, Air | 176 °C |
Deflection Temperature at 1.8 MPa (264 psi) | 305 °C |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.