MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Hexcel® F515 Epoxy Resin, TXX200 Carbon Tape
Categories: Polymer; Thermoset; Carbon Fiber/Thermoset Composite; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes: STD MOD Fiber

Information provided by HexCel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 1482 MPa
@Temperature 71.0 °C
1/2 hr
 1717 MPa
@Temperature 23.0 °C
Tensile Modulus 108.9 GPa
@Temperature 71.0 °C
1/2 hr
 110.3 GPa
@Temperature 23.0 °C
Flexural Yield Strength 1289 MPa
@Temperature 71.0 °C
1/2 hr
 1558 MPa
@Temperature 23.0 °C
Flexural Modulus 124.8 GPa
@Temperature 71.0 °C
1/2 hr
 125.5 GPa
@Temperature 23.0 °C
Compressive Yield Strength 1158 MPa
@Temperature 71.0 °C
1/2 hr
 1303 MPa
@Temperature 23.0 °C
Compressive Modulus 112.4 GPa
@Temperature 71.0 °C
1/2 hr
 117.9 GPa
@Temperature 23.0 °C
Shear Strength 69.6 MPa
@Temperature 71.0 °C
Short Beam, 1/2 hr
 86.9 MPa
@Temperature 23.0 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Hexcel® HexPly® M47 140°C Curing Epoxy Matrix, Woven Carbon Prepreg
Solvay CYCOM® 5276-1 Epoxy with G40-800 Tape Composite
Hexcel® HexPly® 8552 Epoxy Matrix, Carbon Tape Form
Hexcel® HexPly® 8551-7 Epoxy Matrix, AS4 Fiber
Hexcel® HexMC® C/2000/R1A Carbon Epoxy Molding Composite

PHEXC128 / 98598

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.