MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

LyondellBasell Adflex X 500F Thermoplastic Polyolefin
Categories: Polymer; Film; Thermoplastic; Polyolefin

Material Notes: Adflex X 500 F is a thermoplastic polyolefin which is typically used in co-extruded cast film and injection molding applications. Adflex X 500 F features a high softness, a low modulus, high gloss and excellent clarity. It has been selected for use in a central layer of tough transparent co-extruded cast-film structures. It can be blended with other transparent polyolefin resins to improve the low temperature impact resistance maintaining the transparency of the film. Adflex X 500 F can be processed on conventional PP cast film lines. It is also suited for injection molding applications where high transparency and good gloss combined with good flexibility is required like e.g. house wares and toys. It does not contain any slip nor anti-blocking agents.

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.890 g/cc0.0322 lb/in³Method A; ISO 1183-1
Melt Flow 7.5 g/10 min
@Load 2.16 kg,
Temperature 230 °C
7.5 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133-1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 46
@Time 15.0 sec
46
@Time 0.00417 hour
ISO 868
Tensile Strength at Break 22.0 MPa3190 psiISO 527-1,-2
Tensile Strength, Yield 14.0 MPa2030 psiISO 527-1,-2
Elongation at Break 700 %700 %ISO 527-1,-2
Elongation at Yield 20 %20 %ISO 527-1,-2
Flexural Modulus 0.550 GPa79.8 ksiISO 178
Charpy Impact, Notched  0.500 J/cm²
@Temperature -40.0 °C
2.38 ft-lb/in²
@Temperature -40.0 °F
failure mode: complete break; ISO 179
 4.50 J/cm²
@Temperature -20.0 °C
21.4 ft-lb/in²
@Temperature -4.00 °F
failure mode-partial break; ISO 179
 6.50 J/cm²
@Temperature 23.0 °C
30.9 ft-lb/in²
@Temperature 73.4 °F
failure mode-partial break; ISO 179
 
Thermal PropertiesMetricEnglishComments
Melting Point 163 °C325 °FDSC; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 58.0 °C136 °Funannealed; ISO 75B-1,-2
Vicat Softening Point 94.0 °C201 °FA50; ISO 306
 
Optical PropertiesMetricEnglishComments
Haze  13 %
@Thickness 0.0500 mm
13 %
@Thickness 0.00197 in
ASTM D1003
 23 %
@Thickness 1.14 mm
23 %
@Thickness 0.0450 in
ASTM D1003
Gloss  60 %
@Thickness 0.0500 mm
60 %
@Thickness 0.00197 in
@ 45°; ASTM D2457
 110 %
@Thickness 1.14 mm
110 %
@Thickness 0.0450 in
@60°; ASTM D2457
 
Descriptive Properties
Processing MethodCast Film; Extrusion Coating; Injection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
CTC X-PRO CTC PP2020 Polypropylene Impact Copolymer
LyondellBasell Adflex Z 101H Thermoplastic Polyolefin
LyondellBasell Adflex X 100G Thermoplastic Polyolefin
Dow INSPIRE™ D500.00 Performance Polymer

PEQT7004 / 218643

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.