MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Sax Polymers SAXALEN PPC339T20 Polypropylene Copolymer, 20% Talc Filled
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 20% Talc Filler

Material Notes: SAXALEN PPC339T20 is a 20% mineral filled Polypropylene - Copolymer intended for injection molding with good flow properties und higher stiffness. The PP-Copolymer has low warpage behaviors and good surface properties.

Information provided by SAX Polymers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/cc
Melt Flow 12 g/10 min
@Load 2.16 kg,
Temperature 230 °C
from MVR; ISO 1033
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 25.0 MPa50 mm/min; ISO 527-1
Elongation at Break 18 %50mm/min; ISO 527-1
Tensile Modulus 2400 MPa1 mm/min; ISO 527-1
Flexural Strength 33.0 MPa2 mm/min; ISO 178
Flexural Modulus 2000 MPa2 mm/min; ISO 178
Izod Impact, Notched (ISO) 4.00 kJ/m²
@Temperature -30.0 °C
ISO 180/1A
 5.00 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
Izod Impact, Unnotched (ISO) 24.0 kJ/m²
@Temperature -30.0 °C
ISO 180/1U
 55.0 kJ/m²
@Temperature 23.0 °C
ISO 180/1U
Charpy Impact Unnotched 25.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
 50.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 7.00 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C80*10*4 s=60mm; ISO 75-1 a
Vicat Softening Point 75.0 °CB/120; ISO 306
 
Processing PropertiesOriginal ValueComments
Melt Temperature 220 - 250 °C
Mold Temperature 40.0 - 70.0 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polypropylene with 20% Talc Filler
BASF Procom® T20H S63 Polypropylene
BASF Procom® T20C 556 Polypropylene
Sax Polymers SAXALEN PPH335T20 Polypropylene Homopolymer, 20% Talc Filled
Polykemi AB POLYfill PPH TS15010 H VTUV1 Polypropylene Homopolymer, Mineral Reinforced

PSAXP915 / 150864

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.