MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LyondellBasell Alathon® H5112 High Density Polyethylene, Injection Molding Grade
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Injection Molded

Material Notes: ALATHON H5112 is a medium-molecular-weight-distribution resin with balanced impact/ESCR and high flow characteristics. Typical applications include housewares, food containers, pail handles and toys.

Regulatory Status: H5112 meets the requirements of the Food and Drug Administration regulation 21 CFR 177.1520. This regulation allows the use of this olefin polymer in "...articles or components of articles intended for use in contact with food." Specific limitations or conditions of use may apply.

This product is from the former Equistar product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.593 - 0.625 g/ccASTM D1895
Density 0.951 g/ccASTM D1505
Melt Flow 12 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
Spiral Flow 13.8 inEquistar test
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 71ASTM D2240
Tensile Strength at Break 3830 psi50 mm/min; ASTM D638
Elongation at Break 11 %50 mm/min; ASTM D638
Tensile Modulus 105500 psi1% Secant; 50mm/min; ASTM D638
 128200 psi50mm/min; ASTM D638
Flexural Modulus 170400 psi12.5 mm/min; ASTM D790
 131900 psi
@Strain 2 %
Secant; 12.5 mm/min; ASTM D790
Flexural Modulus, 1% Secant 158400 psi2.5 mm/min; ASTM D790
Izod Impact, Notched 0.560 ft-lb/inASTM D256
 NB
@Temperature -18.0 °C
ASTM D4812
 
Thermal PropertiesOriginal ValueComments
Melting Point 262.8 °FASTM D3418
Crystallization Temperature 114.2 °CASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 70.0 °CASTM D648
Vicat Softening Point 124 °CASTM D1525
Brittleness Temperature <= -76.0 °CASTM D746
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 450 °F
Middle Barrel Temperature 470 °F
Front Barrel Temperature 475 °F
Nozzle Temperature 475 °F
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chevron Phillips Marlex® 9004 HDPE Injection Molding Resin
Petromont 3100 High Density Polyethylene Resin
Celanese Hostaform® C 27021 AS POM, Specialty
Celanese Ateva® 1030 Ethylene Vinyl Acetate Copolymer
Celanese Hostaform® C 27021 POM, Unfilled

PEQU0784 / 104140

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.