MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC CYCOLOY™ XCM830 PC+ABS (Europe)
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced

Material Notes: PC/ABS with high stiffness and impact performance

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.22 g/cc1.22 g/ccASTM D792
Density 1.22 g/cc0.0441 lb/in³ISO 1183
Water Absorption 0.40 %0.40 %23°C/sat; ISO 62
Moisture Absorption 0.100 %0.100 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0070 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0070 - 0.0080 in/in
@Thickness 0.126 in
SABIC method
Melt Flow  9.0 g/10 min
@Load 5.00 kg,
Temperature 260 °C
9.0 g/10 min
@Load 11.0 lb,
Temperature 500 °F
cm³/10 min; ISO 1133
 11 g/10 min
@Load 5.00 kg,
Temperature 260 °C
11 g/10 min
@Load 11.0 lb,
Temperature 500 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 55.0 MPa7980 psi5 mm/min; ASTM D638
 55.0 MPa7980 psi5 mm/min; ISO 527
Tensile Strength, Yield 56.0 MPa8120 psi5 mm/min; ISO 527
 60.0 MPa8700 psi5 mm/min; ASTM D638
Elongation at Break 100 %100 %5 mm/min; ISO 527
 100 %100 %5 mm/min; ASTM D638
Elongation at Yield 5.0 %5.0 %5 mm/min; ISO 527
 5.0 %5.0 %5 mm/min; ASTM D638
Tensile Modulus 3.10 GPa450 ksi1mm/min; ISO 527
 3.40 GPa493 ksi5 mm/min; ASTM D638
Flexural Yield Strength 95.0 MPa13800 psi2 mm/min; ISO 178
 95.0 MPa13800 psi1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 3.10 GPa450 ksi2 mm/min; ISO 178
 3.10 GPa450 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 5.00 J/cm9.37 ft-lb/inASTM D256
 1.20 J/cm
@Temperature -30.0 °C
2.25 ft-lb/in
@Temperature -22.0 °F
ASTM D256
Izod Impact, Notched (ISO) 40.0 kJ/m²19.0 ft-lb/in²80*10*4; ISO 180/1A
 10.0 kJ/m²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) NBNB80*10*4; ISO 180/1U
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
80*10*4; ISO 180/1U
Charpy Impact Unnotched NBNBEdgew 80*10*4 sp=62mm; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 4.50 J/cm²21.4 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 1.00 J/cm²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 65.0 J47.9 ft-lbASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
33.3 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
33.3 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
CTE, linear, Transverse to Flow  70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 70.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
38.9 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Thermal Conductivity 0.200 W/m-K1.39 BTU-in/hr-ft²-°FISO 8302
Hot Ball Pressure Test 125 °C257 °FIEC 60695-10-2
Deflection Temperature at 1.8 MPa (264 psi) 118 °C244 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 118 °C
@Thickness 3.20 mm
244 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 138 °C280 °FRate B/50; ASTM D1525
 138 °C280 °FRate B/50; ISO 306
 140 °C284 °FRate B/120; ISO 306
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 260 - 290 °C500 - 554 °FInjection Molding
Zone 1 260 - 270 °C500 - 518 °F
Zone 2 265 - 290 °C509 - 554 °F
Zone 3 270 - 300 °C518 - 572 °F
Melt Temperature 270 - 300 °C518 - 572 °F
Mold Temperature 60.0 - 100 °C140 - 212 °F
Drying Temperature 110 - 120 °C230 - 248 °FInjection Molding
Dry Time 2.00 - 6.00 hour2.00 - 6.00 hourInjection Molding
Moisture Content 0.020 %0.020 %
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 30 - 80 %30 - 80 %
Vent Depth 0.00380 - 0.00760 cm0.00150 - 0.00299 in
Screw Speed 40 - 70 rpm40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI10769 / 244236

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.