MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Celanese Hostaform® C 13021 POM  (Unverified Data**)
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: Chemical abbreviation according to ISO 1043-1: POM
Injection molding grade with moderate flow

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.41 g/cc0.0509 lb/in³ISO 1183
Melt Density 1.20 g/cc
@Temperature >=166 °C
0.0434 lb/in³
@Temperature >=331 °F
Water Absorption 0.65 %0.65 %ISO 62
Linear Mold Shrinkage, Flow 0.020 cm/cm0.020 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.018 cm/cm0.018 in/inISO 294-4
Melt Flow 12 g/10 min
@Load 2.16 kg,
Temperature 190 °C
12 g/10 min
@Load 4.76 lb,
Temperature 374 °F
(MVR) cm³/10min; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 65.0 MPa9430 psi50mm/min; ISO 527-2/1A
Elongation at Break 25 %25 %50mm/min; ISO 527-2/1A
Elongation at Yield 9.0 %9.0 %50mm/min; ISO 527-2/1A
Tensile Modulus 2.90 GPa421 ksi1mm/min; ISO 527-2/1A
Flexural Modulus 2.80 GPa406 ksiISO 178
Charpy Impact Unnotched 15.0 J/cm²71.4 ft-lb/in²ISO 179/1eU
 14.0 J/cm²
@Temperature -30.0 °C
66.6 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.650 J/cm²3.09 ft-lb/in²ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
Tensile Creep Modulus, 1 hour 2500 MPa363000 psiISO 899-1
Tensile Creep Modulus, 1000 hours 1300 MPa189000 psiISO 899-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmIEC 60093
Surface Resistance 1.00e+14 ohm1.00e+14 ohmIEC 60093
Dielectric Constant  4.0
@Frequency 100 Hz
4.0
@Frequency 100 Hz
IEC 60250
 4.0
@Frequency 1e+6 Hz
4.0
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 35.0 kV/mm889 kV/inIEC 60243-1
Dissipation Factor  0.0020
@Frequency 100 Hz
0.0020
@Frequency 100 Hz
IEC 60250
 0.0050
@Frequency 1e+6 Hz
0.0050
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 110 µm/m-°C61.1 µin/in-°FISO 11359-2
Specific Heat Capacity 2.21 J/g-°C0.528 BTU/lb-°FInternal
Thermal Conductivity 0.155 W/m-K1.08 BTU-in/hr-ft²-°FInternal
Melting Point 166 °C331 °F10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 1.8 MPa (264 psi) 106 °C223 °FISO 75-1, -2
Flammability, UL94  HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
UL94
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
UL94
Flame Spread <= 75 mm/min<= 3.0 in/minISO 3795 and FMVSS 302
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 30.0 °C68.0 - 86.0 °F
 80.0 - 120 °C176 - 248 °FCavity temperature
 165 °C329 °FEjection temperature; Internal
Feed Temperature 60.0 - 80.0 °C140 - 176 °F
Zone 1 170 - 180 °C338 - 356 °F
Zone 2 180 - 190 °C356 - 374 °F
Zone 3 190 - 200 °C374 - 392 °F
Zone 4 190 - 210 °C374 - 410 °F
Die Temperature 190 - 210 °C374 - 410 °F
Melt Temperature 190 - 230 °C374 - 446 °F
Mold Temperature 80.0 - 120 °C176 - 248 °F
Drying Temperature 120 - 140 °C248 - 284 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour
Moisture Content 0.15 %0.15 %Necessary low maximum residual
Injection Pressure 60.0 - 120 MPa8700 - 17400 psi
Hold Pressure 60.0 - 120 MPa8700 - 17400 psi
Back Pressure 4.00 MPa580 psi
Screw Speed  70 rpm
@Diameter 55.0 mm
70 rpm
@Diameter 2.17 in
 100 rpm
@Diameter 40.0 mm
100 rpm
@Diameter 1.57 in
 150 rpm
@Diameter 25.0 mm
150 rpm
@Diameter 0.984 in
Hot-Working Temperature 190 - 210 °C374 - 410 °F
 
Descriptive Properties
Injection moldingYes
Injection speedslow-medium
Longer pre-drying times/storageCan be stored in standard conditions until processed.
Pre-dryingDrying is not normally required with proper storage
Processing conditions9988

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHCR287 / 158856

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.