Physical Properties | Original Value | Comments |
---|
Density | 8.73 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Tensile Strength | 803 MPa @Thickness 3.18 mm |
| 848 MPa @Thickness 1.57 mm |
Tensile Strength, Yield | 408 MPa @Strain 0.2 %, Thickness 1.57 mm |
| 421 MPa @Strain 0.2 %, Thickness 3.18 mm |
Elongation at Break | 59 % @Thickness 3.18 mm |
| 59 % @Thickness 1.57 mm |
Modulus of Elasticity | 165 GPa @Temperature 700 °C |
| 173 GPa @Temperature 600 °C |
| 183 GPa @Temperature 500 °C |
| 185 GPa @Temperature 400 °C |
| 193 GPa @Temperature 300 °C |
| 197 GPa @Temperature 200 °C |
| 205 GPa @Temperature 100 °C |
| 207 GPa @Temperature 20.0 °C |
Poissons Ratio | 0.33 @Temperature 600 °C |
| 0.34 @Temperature 400 °C |
| 0.34 @Temperature 20.0 °C |
| 0.35 @Temperature 700 °C |
| 0.37 @Temperature 500 °C |
| 0.37 @Temperature 100 °C |
| 0.37 @Temperature 200 °C |
| 0.38 @Temperature 300 °C |
Fatigue Strength | 410 MPa @# of Cycles 1.00e+7 |
| 500 MPa @# of Cycles 1.00e+6 |
| 690 MPa @# of Cycles 100000 |
Shear Modulus | 61.0 GPa @Temperature 700 °C |
| 65.0 GPa @Temperature 600 °C |
| 67.0 GPa @Temperature 500 °C |
| 69.0 GPa @Temperature 400 °C |
| 70.0 GPa @Temperature 300 °C |
| 72.0 GPa @Temperature 200 °C |
| 75.0 GPa @Temperature 100 °C |
| 77.0 GPa @Temperature 20.0 °C |
Impact Test | 404 J @Temperature -196 °C |
| 405 J @Temperature 20.0 °C |
| 2.70 J @Temperature -196 °C, Treatment Temp. 980 °C |
| 2.70 J @Temperature 20.0 °C, Treatment Temp. 980 °C |
| 3.40 J @Temperature -196 °C, Treatment Temp. 870 °C |
| 8.10 J @Temperature 20.0 °C, Treatment Temp. 870 °C |
| 12.2 J @Temperature -196 °C, Treatment Temp. 760 °C |
| 25.1 J @Temperature 20.0 °C, Treatment Temp. 760 °C |
| 400 J @Temperature 20.0 °C, Treatment Temp. 540 °C |
| 401 J @Temperature 20.0 °C, Treatment Temp. 650 °C |
| 403 J @Temperature -196 °C, Treatment Temp. 650 °C |
| 405 J @Temperature -196 °C, Treatment Temp. 540 °C |
|
Electrical Properties | Original Value | Comments |
---|
Electrical Resistivity | 744.4 ohm-cir-mil/ft |
Magnetic Permeability | 1.0001 |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 11.97 µm/m-°C @Temperature 21.0 - 100 °C |
| 12.22 µm/m-°C @Temperature 21.0 - 200 °C |
| 12.56 µm/m-°C @Temperature 21.0 - 300 °C |
| 12.87 µm/m-°C @Temperature 21.0 - 400 °C |
| 13.01 µm/m-°C @Temperature 21.0 - 500 °C |
| 13.18 µm/m-°C @Temperature 21.0 - 600 °C |
Specific Heat Capacity | 0.364 J/g-°C @Temperature -15.0 °C |
| 0.373 J/g-°C @Temperature 20.0 °C |
| 0.389 J/g-°C @Temperature 100 °C |
| 0.410 J/g-°C @Temperature 200 °C |
| 0.431 J/g-°C @Temperature 300 °C |
| 0.456 J/g-°C @Temperature 400 °C |
| 0.477 J/g-°C @Temperature 500 °C |
| 0.498 J/g-°C @Temperature 600 °C |
| 0.519 J/g-°C @Temperature 700 °C |
Thermal Conductivity | 9.80 W/m-K @Temperature 25.0 °C |
| 12.8 W/m-K @Temperature 200 °C |
| 16.6 W/m-K @Temperature 400 °C |
| 21.4 W/m-K @Temperature 600 °C |
| 25.3 W/m-K @Temperature 800 °C |
| 29.6 W/m-K @Temperature 1000 °C |
| 32.6 W/m-K @Temperature 1150 °C |
Melting Point | 1338 - 1380 °C |
Solidus | 1338 °C |
Liquidus | 1380 °C |
|
Processing Properties | Original Value | Comments |
---|
Annealing Temperature | 1180 - 1200 °C |
Hot-Working Temperature | 870 - 1230 °C |
|
Component Elements Properties | Original Value | Comments |
---|
Carbon, C | <= 0.010 % |
Chromium, Cr | 19 - 23 % |
Iron, Fe | <= 2.0 % |
Manganese, Mn | <= 0.75 % |
Molybdenum, Mo | 15 - 17 % |
Nickel, Ni | 52.5 - 63 % |
Phosphorus, P | <= 0.040 % |
Silicon, Si | <= 0.080 % |
Sulfur, S | <= 0.020 % |
Titanium, Ti | 0.020 - 0.25 % |
Tungsten, W | 3.0 - 4.4 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.