MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

EMS-Grivory Grivory® HT2C-3X black 9833 PA6T/66-CF30
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66

Material Notes: Product description: Grivory HT2C-3X black 9833 us a 30% carbon-fiber reinforced engineering thermoplastic material based on a semi-crystalline, partially aromatic copolyamide. Acc to ISO: PA 6T/66. Acc. to ASTM: PPA, polyphthalamide. Grivory HT2C-3X black 9833 is an injection molding material which has a low density. It is electrically conductive. The main distinguishing feature of Grivory HT, when compared to other polyamides, is its good performance at high temperatures providing parts which are stiffer, stronger and have better heat distortion stability and chemical resistance. Grivory HT is suitable for production of technical parts in the application fields of:
  • Electrical/Electronics
  • Automotive
  • Safety technology
  • Mechanical engineering

Information provided by EMS Grivory

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.32 g/cc0.0477 lb/in³Dry; ISO 1183
Water Absorption 4.5 %4.5 %Sim. to ISO 62
Moisture Absorption 1.50 %1.50 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0010 cm/cm0.0010 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0050 cm/cm0.0050 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 290 MPa42100 psiConditioned; ISO 2039-1
 300 MPa43500 psiDry; ISO 2039-1
Tensile Strength at Break 265 MPa38400 psiConditioned; ISO 527-1/-2
 275 MPa39900 psiDry; ISO 527-1/-2
Elongation at Break 2.0 %2.0 %Dry; ISO 527-1/-2
 2.0 %2.0 %Conditioned; ISO 527-1/-2
Tensile Modulus 24.0 GPa3480 ksiConditioned; ISO 527-1/-2
 24.5 GPa3550 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  5.00 J/cm²
@Temperature -30.0 °C
23.8 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eU
 5.00 J/cm²
@Temperature -30.0 °C
23.8 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 5.50 J/cm²
@Temperature 23.0 °C
26.2 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eU
 5.50 J/cm²
@Temperature 23.0 °C
26.2 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
Charpy Impact, Notched  0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 0.800 J/cm²
@Temperature 23.0 °C
3.81 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 0.800 J/cm²
@Temperature 23.0 °C
3.81 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 50 ohm-cm50 ohm-cmDry; IEC 60093
 50 ohm-cm50 ohm-cmConditioned; IEC 60093
Surface Resistance 100 ohm100 ohmIEC 60093
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 15.0 µm/m-°C8.33 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 75.0 µm/m-°C41.7 µin/in-°FISO 11359-1/-2
Melting Point 310 °C590 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 140 °C284 °FLong Term; ISO 2578
 270 °C518 °FShort Term; EMS
Deflection Temperature at 1.8 MPa (264 psi) 290 °C554 °FISO 75-1/-2
Deflection Temperature at 8.0 MPa 245 °C473 °FISO 75-1/-2
Flammability, UL94 HBHBIEC 60695-11-10
 
Descriptive Properties
AutomotiveCompressed air systems
 Fuel systems
 Hydraulic systems
 Interior
 Powertrain and Chassis
Electricals & ElectronicsElectrical equipment
FormGranules
Industry & Consumer goodsHousewares
 Hydraulics & Pneumatics
 Mechanical Engineering
 Power transmission
 Tools & Accessories
ProcessingInjection Molding
Product AttributesCo Polyamide
 Improved alcohol resistance
 Improved friction & wear properties
 Partially aromatic Polyamide
Special CharacteristicsAnti-static
 Improved heat resistance

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 66, 10% Carbon Fiber Filled
EMS-Grivory Grilon® TSC-30/4 EC black 9832 PA666-CF30
EMS-Grivory Grilon® TSC-30/4 LF 15 black 9832 PA666-(CF+Z)45
Overview of materials for Nylon 66, 30% Carbon Fiber Filled
A. Schulman ComAlloy Lubrilon® 646 Nylon 6/12, Carbon Fiber/PTFE Reinforced

PGRH380 / 157089

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.