MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
MicroFine™ Protoyping Resin
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer

Material Notes: Proto Labs' MicroFine™ material is available in opaque green and gray. It is an ABS-like material that is formulated for micro-resolution stereolithography applications. MicroFine enables the production of parts with the finest features and tightest tolerances in the industry. Its mechanical properties make it a durable choice for small part applications.

Information provided by Proto Labs.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Water Absorption 0.9 %ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 85ASTM D2240M
Tensile Strength at Break 60.0 MPaASTM D638M
Elongation at Break 8.0 %ASTM D638M
Tensile Modulus 2.60 GPaASTM D638M
Flexural Strength 74.3 MPaASTM D790M
Flexural Modulus 2.20 GPaASTM D790M
Izod Impact, Notched 0.230 J/cmASTM D256A
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 2.94
@Frequency 1e+6 Hz
ASTM D150-98
 3.12
@Frequency 1000 Hz
ASTM D150-98
 3.16
@Frequency 60 Hz
ASTM D150-98
Dielectric Strength 14.89 kV/mmASTM D149-97a
 
Thermal PropertiesOriginal ValueComments
CTE, linear 74.1 µm/m-°C
@Temperature -40.0 - 0.000 °C
ASTM E831-05
 96.3 µm/m-°C
@Temperature 0.000 - 50.0 °C
ASTM E831-05
 141.8 µm/m-°C
@Temperature 50.0 - 100 °C
ASTM E831-05
 182 µm/m-°C
@Temperature 100 - 150 °C
ASTM E831-05
Deflection Temperature at 0.46 MPa (66 psi) 59.0 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 50.0 °CASTM D648
Glass Transition Temp, Tg 49.0 °CASTM E15145-00

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
3D Systems RenShape® SL 7820 Stereolithography Plastic
DSM Somos® PerFORM Stereolithography Polymer, UV Postcure
3D Systems Accura® 60 Plastic for SLA® Systems
3D Systems DuraForm® EX Impact-Resistant Plastic for SLS® Systems
3D Systems DuraForm® PA Nylon for SLS® Systems

PPROTL990 / 191504

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.