MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AGC AFLAS® 100H TFE/P Fluoroelastomers
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: Description: AFLAS® Fluoroelastomers are copolymers of tetrafluoroethylene and propylene. This combination gives AFLAS Fluoroelastomers unique properties over conventional FKM-type fluoroelastomers in demanding applications found in the oil & gas, chemical process, industrial equipment, food handling, pharmaceutical, heavy duty diesel and automotive industries. AFLAS Fluoroelastomers display outstanding resistance to heat, acids and bases, many solvents, ozone, and steam. Classified by ASTM D 1418-01 as FEPM.

Material Features:

    High molecular weight
  • Outstanding elongation, even in formulations with high hardness
  • Excellent base and amine resistance unmatched by FKM-type fluoroelastomer
  • High heat resistance
  • Outstanding steam resistance
End User Benefits:
    Preferred material for high pressure and high temperature (HPHT) in oil & gas applications
  • Long service use (> 25 years) in harsh environments
  • Can be compounded to be highly resistant to rapid gas decompression (e.g. NORSOK)
  • Chemical durability (e.g. oil exploration and production fluids)
Typical Applications:
    O-rings
  • Gaskets
  • Oilfield parts
  • Heavy Duty seals

Information provided by AGC Chemicals Americas Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 21.0 MPa3050 psi
 17.85 MPa
@Treatment Temp. 175 °C,
Time 2.59e+6 sec
2589 psi
@Treatment Temp. 347 °F,
Time 720 hour
SM class Engine Oil Resistance
 17.85 MPa
@Treatment Temp. 150 °C,
Time 3.60e+6 sec
2589 psi
@Treatment Temp. 302 °F,
Time 1000 hour
IRM 903 Oil Resistance
 18.27 MPa
@Treatment Temp. 180 °C,
Time 2.59e+6 sec
2650 psi
@Treatment Temp. 356 °F,
Time 720 hour
Steam Resistance
 18.9 MPa
@Treatment Temp. 200 °C,
Time 3.60e+6 sec
2740 psi
@Treatment Temp. 392 °F,
Time 1000 hour
Heat Resistance
 21.63 MPa
@Treatment Temp. 70.0 °C,
Time 2.59e+6 sec
3137 psi
@Treatment Temp. 158 °F,
Time 720 hour
50% NaOH Resistance
Elongation at Break 300 %300 %
 282 %
@Treatment Temp. 70.0 °C,
Time 2.59e+6 sec
282 %
@Treatment Temp. 158 °F,
Time 720 hour
50% NaOH Resistance
 315 %
@Treatment Temp. 175 °C,
Time 2.59e+6 sec
315 %
@Treatment Temp. 347 °F,
Time 720 hour
SM class Engine Oil Resistance
 315 %
@Treatment Temp. 180 °C,
Time 2.59e+6 sec
315 %
@Treatment Temp. 356 °F,
Time 720 hour
Steam Resistance
 327 %
@Treatment Temp. 150 °C,
Time 3.60e+6 sec
327 %
@Treatment Temp. 302 °F,
Time 1000 hour
IRM 903 Oil Resistance
 363 %
@Treatment Temp. 200 °C,
Time 3.60e+6 sec
363 %
@Treatment Temp. 392 °F,
Time 1000 hour
Heat Resistance
Tensile Modulus 0.000500 GPa0.0725 ksiG' Storage Modulus (nominal) of Raw Gum
100% Modulus 6.00 MPa
@Strain 100 %
870 psi
@Strain 100 %
Compression Set 30 %
@Temperature 200 °C,
Time 252000 sec
30 %
@Temperature 392 °F,
Time 70.0 hour
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -40.0 °C-40.0 °FBrittle Point
 3.00 °C37.4 °FTR-10
Glass Transition Temp, Tg -3.00 °C26.6 °F
 
Processing PropertiesMetricEnglishComments
Cure Time  4.60 min
@Temperature 177 °C
0.0767 hour
@Temperature 351 °F
90% cure, 100CPM, 3° Strain, 12 minutes
 13.0 min
@Temperature 177 °C
0.217 hour
@Temperature 351 °F
50% cure, tc50, 100CPM, 3° Strain, 12 minutes
 20.0 min
@Temperature 170 °C
0.333 hour
@Temperature 338 °F
Press
 240 min
@Temperature 200 °C
4.00 hour
@Temperature 392 °F
Post cure
 
Component Elements PropertiesMetricEnglishComments
Fluorine, F 57 %57 %
 
Descriptive Properties
Cure Data11.9 dNmMin S'
 49.8 dNmMax S'
Volume Change (%)-0.0150% NaOH Resistance 70°C for 720 hours
 13.4IRM 903 Oil Resistance 150°C for 1000 hours
 5SM class Engine Oil Resistance 175°C for 720 hours

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AGC AFLAS® 100S TFE/P Fluoroelastomers
Natural Rubber, Vulcanized (NR, IR, Polyisoprene)
ATG s.r.l. FVMQ Fluorosilicone Rubber
Fluorosilicone Rubber (FMQ, FVMQ, FSi)
Dow Silastic® LS 4-9040 FLUOROSILICONE RUBBER

PAGCX011 / 191120

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.