Physical Properties | Original Value | Comments |
---|
Density | 1.00 - 1.55 g/cc |
Filler Content | 5.00 - 20.0 % |
Water Absorption | 0.0100 - 0.300 % |
Moisture Absorption at Equilibrium | 0.100 - 0.340 % |
Water Absorption at Saturation | 0.120 - 0.500 % |
Water Vapor Transmission | 15.0 g/m²/day |
Oxygen Transmission | 65.0 - 3150 cc-mm/m²-24hr-atm |
Nitrogen Transmission | 12.0 - 630 cc-mm/m²-24hr-atm |
Carbon Dioxide Transmission | 380 - 18900 cc-mm/m²-24hr-atm |
Viscosity | 240000 - 640000 cP @Temperature 260 - 260 °C |
| 240000 - 640000 cP @Frequency 1000 - 1000 Hz |
Maximum Moisture Content | 0.0200 - 0.0400 |
| 0.200 - 0.200 @Temperature 120 - 120 °C |
| 0.200 - 0.200 @Time 299 - 299 sec |
Linear Mold Shrinkage | 0.00100 - 0.0120 cm/cm |
| 0.00700 - 0.00700 cm/cm @Temperature 80.0 - 80.0 °C |
Linear Mold Shrinkage, Transverse | 0.00200 - 0.00800 cm/cm |
| 0.00700 - 0.00700 cm/cm @Temperature 80.0 - 80.0 °C |
Melt Flow | 2.00 - 60.0 g/10 min |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Rockwell M | 50.0 - 118 |
Hardness, Rockwell R | 90.0 - 123 |
Ball Indentation Hardness | 111 - 116 MPa |
Tensile Strength, Ultimate | 34.0 - 228 MPa |
| 35.0 - 35.0 MPa @Temperature 60.0 - 60.0 °C |
Tensile Strength, Yield | 48.3 - 125 MPa |
Elongation at Break | 1.40 - 150 % |
| 70.0 - 70.0 % @Temperature 60.0 - 120 °C |
Elongation at Yield | 2.00 - 130 % |
| 2.50 - 6.00 % @Temperature 60.0 - 120 °C |
Modulus of Elasticity | 0.225 - 10.0 GPa |
| 1.70 - 2.20 GPa @Temperature 60.0 - 120 °C |
Flexural Yield Strength | 9.81 - 160 MPa |
Flexural Modulus | 0.228 - 7.90 GPa |
Flexural Strain at Yield | 7.00 - 7.20 % |
Compressive Yield Strength | 75.0 - 86.2 MPa |
Izod Impact, Notched | 0.343 - 9.61 J/cm |
| 1.00 - 7.00 J/cm @Temperature -40.0 - 0.000 °C |
| >= 1.1768 J/cm @Temperature -30.0 - -30.0 °C |
| >= 1.1768 J/cm @Thickness 3.20 - 3.20 mm |
Izod Impact, Unnotched | 7.35 J/cm - NB |
| NB - NB @Temperature -40.0 - -40.0 °C |
Izod Impact, Notched (ISO) | 6.00 - 90.0 kJ/m² |
| 8.00 - 20.0 kJ/m² @Temperature -30.0 - -30.0 °C |
| 8.00 - 16.0 kJ/m² @Temperature -30.0 - -30.0 °C |
| 8.00 - 16.0 kJ/m² @Thickness 3.00 - 76.2 mm |
Izod Impact, Unnotched (ISO) | 43.0 kJ/m² - NB |
| NB - NB @Temperature -30.0 - -30.0 °C |
Charpy Impact Unnotched | 3.50 J/cm² - NB |
| 30.0 J/cm² - NB @Temperature -60.0 - -20.0 °C |
Charpy Impact, Notched | 0.600 - 10.0 J/cm² |
| 0.700 - 4.50 J/cm² @Temperature -40.0 - -20.0 °C |
| 1.20 - 1.80 J/cm² @Temperature -30.0 - -30.0 °C |
| 1.20 - 1.80 J/cm² @Thickness 3.00 - 3.00 mm |
Gardner Impact | 36.0 - 36.2 J |
Tensile Impact Strength | 378 - 631 kJ/m² |
Instrumented Impact Total Energy | 62.2 - 93.8 J |
Puncture Energy | 45.0 - 81.3 J |
| 50.0 - 88.1283 J @Temperature -30.0 - -30.0 °C |
Tensile Creep Modulus, 1 hour | 2100 - 5900 MPa |
Tensile Creep Modulus, 1000 hours | 1700 - 5400 MPa |
|
Electrical Properties | Original Value | Comments |
---|
Electrical Resistivity | 1.00e+12 - 2.00e+18 ohm-cm |
| 3.00e+15 - 3.00e+15 ohm-cm @Temperature 90.0 - 90.0 °C |
Surface Resistance | 100 - 1.00e+17 ohm |
Dielectric Constant | 2.80 - 3.20 |
Dielectric Strength | 15.0 - 41.0 kV/mm |
Dissipation Factor | 0.000100 - 0.0100 |
Arc Resistance | 0.000 - 420 sec |
Comparative Tracking Index | 50.0 - 600 V |
Hot Wire Ignition, HWI | 15.0 - 120 sec |
High Amp Arc Ignition, HAI | 15.0 - 142 arcs |
High Voltage Arc-Tracking Rate, HVTR | 10.0 - 150 mm/min |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 23.4 - 117 µm/m-°C |
CTE, linear, Transverse to Flow | 60.0 - 80.0 µm/m-°C |
Specific Heat Capacity | 1.13 - 2.10 J/g-°C |
Thermal Conductivity | 0.187 - 0.260 W/m-K |
Melting Point | 230 - 280 °C |
Maximum Service Temperature, Air | 60.0 - 120 °C |
Hot Ball Pressure Test | 123 - 140 °C |
Deflection Temperature at 0.46 MPa (66 psi) | 93.0 - 174 °C |
Deflection Temperature at 1.8 MPa (264 psi) | 69.0 - 230 °C |
Vicat Softening Point | 97.0 - 185 °C |
Heat Distortion Temperature | 132 - 135 °C |
Glass Transition Temp, Tg | 80.0 - 149 °C |
UL RTI, Electrical | 80.0 - 140 °C |
UL RTI, Mechanical with Impact | 80.0 - 130 °C |
UL RTI, Mechanical without Impact | 80.0 - 140 °C |
Flammability, UL94 | HB - 5VA |
Flash Point | 430 - 550 °C |
Oxygen Index | 26.0 - 37.6 % |
Glow Wire Test | 750 - 960 °C |
|
Optical Properties | Original Value | Comments |
---|
Refractive Index | 1.57 - 1.59 |
Haze | 0.500 - 88.0 % |
Transmission, Visible | 0.000 - 93.0 % |
UV Transmittance | 85.0 % |
|
Processing Properties | Original Value | Comments |
---|
Processing Temperature | 70.0 - 300 °C |
Nozzle Temperature | 240 - 332 °C |
Melt Temperature | 220 - 343 °C |
Mold Temperature | 40.0 - 121 °C |
Injection Velocity | 40.0 - 240 mm/sec |
Drying Temperature | 60.0 - 130 °C |
Moisture Content | 0.0200 - 0.200 % |
Dew Point | -40.0 - -17.8 °C |
Injection Pressure | 4.96 - 152 MPa |
Vent Depth | 0.00127 - 0.00800 cm |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.