MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Elastron® Elastron® G F.G401.A40.N SEBS
Categories: Polymer; Thermoplastic; Styrene-Butadiene

Material Notes: Product Description: A soft, colorable SEBS based thermoplastic elastomer (TPE) compound designed for contact with non-fatty foods. The monomers and additives used to produce this product are listed in the Union List of Authorized Substances of Regulation 10/20/11/EC. Bondable to: PP, EVA, PE
Availability: Africa & Middle East; Asia Pacific; Europe; North America
Features: Block Copolymer; Bondability; Food Contact Acceptable; Good Colorability; Soft
Agency Ratings: EU 2011/10/EC
RoHS Compliance: RoHS Compliant
Appearance: Natural Color
Forms: Pellets
Processing Method: Injection Molding

Information provided by Elastron

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.882 g/cc0.0319 lb/in³ASTM D792
Linear Mold Shrinkage, Flow 0.033 cm/cm0.033 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.012 cm/cm0.012 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 4040ASTM D2240
Tensile Strength at Break 5.50 MPa798 psiASTM D412
Tensile Stress  0.903 MPa
@Strain 100 %
131 psi
@Strain 100 %
ASTM D412
 1.70 MPa
@Strain 300 %
247 psi
@Strain 300 %
ASTM D412
Elongation at Break 1200 %1200 %ASTM D412
Tear Strength 24.0 kN/m137 pliASTM D624
Compression Set  14 %
@Temperature 22.8 °C,
Time 79200 sec
14 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 36 %
@Temperature 70.0 °C,
Time 79200 sec
36 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395
 61 %
@Temperature 100 °C,
Time 79200 sec
61 %
@Temperature 212 °F,
Time 22.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 145 - 175 °C293 - 347 °F
Middle Barrel Temperature 155 - 185 °C311 - 365 °F
Front Barrel Temperature 160 - 190 °C320 - 374 °F
Nozzle Temperature 175 - 205 °C347 - 401 °F
Zone 1 150 - 170 °C302 - 338 °F
Zone 2 155 - 175 °C311 - 347 °F
Zone 3 165 - 185 °C329 - 365 °F
Zone 4 175 - 205 °C347 - 401 °F
Zone 5 180 - 210 °C356 - 410 °F
Die Temperature 190 - 210 °C374 - 410 °F
Mold Temperature 25.0 - 50.0 °C77.0 - 122 °F
 
Descriptive Properties
Ozone ResistanceNo CracksStressed, ASTM D518
Suggested Max Regrind0.2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PELAST200 / 267782

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.