MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Thermx® TE3002 BK010 PCT
Categories: Polymer; Thermoplastic; Polyester, TP; Polycyclohexylenedimethylene Terephthalate (PCT); Polycyclohexylenedimethylene Terephthalate (PCT), 30% Glass Reinforced

Material Notes: Thermx® TE3002 BK010 is a 30% glass fiber reinforced, flame retardant, black high performance polyester resin for injection molding.

Celenese acquired the Thermx product line from DuPont in 2010.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.65 g/ccISO 1183
Filler Content 30 %
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 100 MPaISO 527
Elongation at Break 1.2 %ISO 527
Tensile Modulus 10000 MPa
@Temperature 23.0 °C
ISO 527
Flexural Strength 150 MPaISO 178
Flexural Modulus 10500 MPaISO 178
Charpy Impact Unnotched 2.00 J/cm²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 0.700 J/cm²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 240 °CISO 75-1/-2
UL RTI, Electrical 150 °C
@Thickness 1.50 mm
UL 746B
 150 °C
@Thickness 0.790 mm
UL 746B
 150 °C
@Thickness 3.00 mm
UL 746B
UL RTI, Mechanical without Impact 140 °C
@Thickness 0.790 mm
UL 746B
 150 °C
@Thickness 3.00 mm
UL 746B
 150 °C
@Thickness 1.50 mm
UL 746B
Flammability, UL94 V-0
@Thickness 0.790 mm
IEC 60695-11-10
 V-0
@Thickness 1.50 mm
IEC 60695-11-10
 V-0
@Thickness 0.790 mm
UL94
 V-0
@Thickness 1.50 mm
UL94
 V-0
@Thickness 3.00 mm
IEC 60695-11-10
 V-0
@Thickness 3.00 mm
UL94
 
Processing PropertiesOriginal ValueComments
Melt Temperature 300 °COptimum
 295 - 310 °C
Mold Temperature 100 °COptimum
 80.0 - 120 °C
Drying Temperature 95.0 °C
Dry Time 4 - 6 hourDehumidified Dryer
Moisture Content <= 0.030 %
 
Descriptive Properties
ColorBlack
Drying RecommendedYes
FillerGlass Reinforced
FormsPellets
GenericPCT
Part Marking Code>PCT-GF30FR(17)<ISO 11469
Polymer FamilyPolyester
Polymer TypePCT
Processing MethodInjection Molding
Product CategoryFlame Retardant Resins
 Glass Reinforced Resins
Region AvailableAmericas
 Asia/Pacific
 Europe
Resin IdentificationPCT-GF30FR(17)ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Thermx® CG023 NC010 PCT
Celanese Thermx® TE1001 BK010 PCT
Celanese Thermx® CG923 BK010 PCT
Celanese Thermx® LED 0201 PCT, 40% Specialty
Celanese Thermx® LED 0201S PCT, 38% Specialty

PDTA7740 / 89901

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.