MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV 4175 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 4100 series are engineered materials designed primarily for demanding automotive and industrial applications. Available in both black and natural, this product is a low density, medium hardness thermoplastic vulcanizate that exhibits excellent compression set, flex fatigue, high and low temperature performance. The material can be processed by injection molding, blow molding and extrusion for applications such as seals, gaskets, chemical resistant hose and tube, boots and bellows.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Excellent Elastic Recovery; Fatigue Resistant; Good Adhesion; Good Flexibility; Good Melt Strength; Good Moldability; Good Processability; Good Surface Finish; High Melt Stability; Low Density; Low Specific Gravity; Medium Hardness; Medium Heat Resistant; Resilient

Uses: Agricultural Applications; Appliance Components; Automotive Applications; Automotive Interior Parts; Automotive Under the Hood; Blow Molding Applications; Gaskets; Hose; Industrial Applications; Pipe Seals; Profiles; Rubber Replacement; Seals; White Goods & Small Appliance

Agency Ratings: UL 94

RoHS Compliance: RoHS Compliant

Automotive Specifications: CHRYSLER MS-AR-100 CGN Color: Black; CHRYSLER MS-AR-100 CGN Color: Natural; FORD WSD-M2D379-A1 Color: Black; FORD WSD-M2D380-A1 Color: Black; FORD WSD-M2D380-A1 Color: Natural; GM GMP.E/P.003 Color: Black; GM GMP.E/P.003 Color: Natural; GM GMW/15813 Type 6 Color: Black; GM GMW/15813 Type 6 Color: Natural; GM QK 3523 L Color: Black; GM QK 3523 L Color: Natural; PSA Peugeot-Citroen B62 0300 version G Color: Black

UL File Number: QMFZ2. E54709

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.960 g/cc0.0347 lb/in³ISO 1183
Viscosity 340 cP
@Shear Rate 206 1/s,
Temperature 200 °C
340 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  72
@Time 5.00 sec
72
@Time 0.00139 hour
Extruded; ASTM D2240
 75
@Time 5.00 sec
75
@Time 0.00139 hour
Injection Molded; ASTM D2240
Tensile Strength 7.17 MPa1040 psiFlow; ISO 37
 8.48 MPa1230 psiAcross Flow; ISO 37
 7.72 MPa
@Thickness 4270 mm,
Temperature 150 °C
1120 psi
@Thickness 168 in,
Temperature 302 °F
Across Flow, Change in Air; ISO 188
 8.31 MPa
@Thickness 25400 mm,
Temperature 135 °C
1210 psi
@Thickness 1000 in,
Temperature 275 °F
Across Flow, Change in Air; ISO 188
Tensile Stress at Strain  3.30 MPa
@Strain 100 %
479 psi
@Strain 100 %
Across Flow; ISO 37
 5.30 MPa
@Strain 100 %
769 psi
@Strain 100 %
Flow; ISO 37
 3.40 MPa
@Strain 100 %,
Treatment Temp. 135 °C
493 psi
@Strain 100 %,
Treatment Temp. 275 °F
Across Flow, Change in Air at 1000 hr; ISO 188
 3.47 MPa
@Strain 100 %,
Treatment Temp. 150 °C
503 psi
@Strain 100 %,
Treatment Temp. 302 °F
Across Flow, Change in Air at 168 hr; ISO 188
Elongation at Break 300 %300 %Flow; ASTM D412
 590 %590 %Across Flow; ASTM D412
 496 %
@Treatment Temp. 150 °C,
Time 605000 sec
496 %
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
 561 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
561 %
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
Tear Strength 38.6 kN/m220 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set  22 %
@Temperature 22.8 °C,
Time 79200 sec
22 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 31 %
@Temperature 70.0 °C,
Time 79200 sec
31 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 45 %
@Temperature 125 °C,
Time 252000 sec
45 %
@Temperature 257 °F,
Time 70.0 hour
ISO 815
 
Thermal PropertiesMetricEnglishComments
UL RTI, Electrical 100 °C212 °FUL 746
UL RTI, Mechanical with Impact 65.0 °C149 °FUL 746
UL RTI, Mechanical without Impact 100 °C212 °FUL 746
Flammability, UL94 HB
@Thickness 1.02 mm
HB
@Thickness 0.0400 in
All Colors
 
Processing PropertiesMetricEnglishComments
Processing Temperature 182 - 227 °C360 - 440 °FInjection
Rear Barrel Temperature 138 - 160 °C280 - 320 °FInjection
Middle Barrel Temperature 166 - 193 °C330 - 380 °FInjection
Front Barrel Temperature 177 - 227 °C350 - 440 °FInjection
Nozzle Temperature 182 - 227 °C360 - 440 °FInjection
Zone 1 180 - 200 °C356 - 392 °FExtrusion
Zone 2 180 - 205 °C356 - 401 °FExtrusion
Zone 3 187 - 210 °C369 - 410 °FExtrusion
Zone 4 187 - 210 °C369 - 410 °FExtrusion
Die Temperature 195 - 215 °C383 - 419 °FExtrusion
Melt Temperature 195 - 215 °C383 - 419 °FExtrusion
Mold Temperature 15.6 - 54.4 °C60.0 - 130 °FInjection
Drying Temperature 82.2 °C180 °F
Dry Time 3.00 hour3.00 hour
Screw Speed 25 - 75 rpm25 - 75 rpmInjection
 
Descriptive Properties
AppearanceBlack
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Sarlink® TPV 4139D Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 6775N Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 6765N Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 4165 Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 4155 Thermoplastic Vulcanizate

PTEKNQ1159 / 237650

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.