MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Telcar® TL-1934A BLK 111 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes:

Information Provided by Teknor Apex

Key Words: TPE
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.00 g/cc1.00 g/ccASTM D792
Melt Flow 18 g/10 min
@Load 5.00 kg,
Temperature 200 °C
18 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8383ASTM D2240
Tensile Strength at Break 15.5 MPa2250 psiASTM D412
Elongation at Break 630 %630 %ASTM D412
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 2.36
@Frequency 1000 Hz
2.36
@Frequency 1000 Hz
ASTM D150
Dissipation Factor 0.00010
@Frequency 1000 Hz
0.00010
@Frequency 1000 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -60.0 °C-76.0 °FASTM D746
Oxygen Index 18 %18 %ASTM D2863
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 171 - 193 °C340 - 380 °F
Middle Barrel Temperature 177 - 199 °C350 - 390 °F
Front Barrel Temperature 182 - 204 °C360 - 400 °F
Nozzle Temperature 188 - 210 °C370 - 410 °F
Zone 1 166 - 188 °C330 - 370 °F
Zone 2 171 - 193 °C340 - 380 °F
Zone 3 177 - 199 °C350 - 390 °F
Zone 5 182 - 204 °C360 - 400 °F
Die Temperature 190 - 210 °C374 - 410 °F
Melt Temperature 188 - 210 °C370 - 410 °FProcessing Temperature
Mold Temperature 25.0 - 65.6 °C77.0 - 150 °F
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psi
Back Pressure 0.172 - 0.345 MPa25.0 - 50.0 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 100 rpm50 - 100 rpm
 
Descriptive Properties
AppearanceBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Telcar® TL-1934F Styrenic Thermoplastic Elastomer
Teknor Apex Medalist® MD-8431 Thermoplastic Elastomer
Teknor Apex Elexar® EL-8730A Thermoplastic Elastomer
Teknor Apex Elexar® EL-8452 Thermoplastic Elastomer
Teknor Apex ELEXAR® EL 8451 Thermoplastic Elastomer

PTEKNP421 / 129502

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.