MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Morgan Advanced Ceramics Firelite 14 Thermal Ceramic
Categories: Ceramic; Oxide

Material Notes: Porous Aggregate. Hydraulic bond. Insulating castable for service up to 1100°C/2010°F. Combines good strength and low thermal conductivity. Particularly recommended for convection zone, ducts and stacks in petrochemical heaters. Can be used in applications similar to those described by UOP 2-17-0. Conforms to class Q, ASTM classification C-401-84.

Information provided by Morgan Advanced Materials

Key Words: Thermal Ceramics
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 1.20 g/cc0.0434 lb/in³dried to 110°C
Grain Size <= 8000 µm<= 8000 µm
 
Mechanical PropertiesMetricEnglishComments
Compressive Strength 3.90 MPa566 psiCold Crushing Strength, MST
 5.90 MPa
@Treatment Temp. 815 °C
856 psi
@Treatment Temp. 1500 °F
Cold Crushing Strength
 8.80 MPa
@Treatment Temp. 110 °C
1280 psi
@Treatment Temp. 230 °F
Cold Crushing Strength
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  0.210 W/m-K
@Temperature 200 °C
1.46 BTU-in/hr-ft²-°F
@Temperature 392 °F
ASTM C 417
 0.240 W/m-K
@Temperature 400 °C
1.67 BTU-in/hr-ft²-°F
@Temperature 752 °F
ASTM C 417
 0.270 W/m-K
@Temperature 600 °C
1.87 BTU-in/hr-ft²-°F
@Temperature 1110 °F
ASTM C 417
Maximum Service Temperature, Air <= 1100 °C<= 2010 °F
Shrinkage 0.20 %0.20 %MST
 0.20 %
@Treatment Temp. 815 °C
0.20 %
@Treatment Temp. 1500 °F
 
Component Elements PropertiesMetricEnglishComments
Al2O3 31.4 %31.4 %
CaO 19.8 %19.8 %
Fe2O3 7.2 %7.2 %
K2O+Na2O 3.7 %3.7 %Na2O + K2O
SiO2 36 %36 %
TiO2 1.4 %1.4 %
 
Descriptive Properties
Net Material Required (kg/m³)1060
Water Addition36% by weight, 25kg bag weight.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

CMORF6314 / 203098

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.