MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

BRP Manufacturing BA615 EPDM Rubber Sheet
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Material: EPDM Rubber Sheet
BRP Style: BA615
Finish: Smooth (Fabric Finish is Available)
ASTM Callout: ASTM D2000 3BA615A14B13C12C20F19P2Z, Z= FMV-SS-302

Information provided by BRP Manufacturing Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength >= 10.3 MPa>= 1500 psiOriginal; ASTM D412
 <= 7.757 MPa
@Temperature 100 °C,
Time 252000 sec
<= 1125 psi
@Temperature 212 °F,
Time 70.0 hour
A14 – Heat Resistance; ASTM D573
 7.24 - 13.4 MPa
@Temperature 100 °C,
Time 252000 sec
1050 - 1950 psi
@Temperature 212 °F,
Time 70.0 hour
Heat Aged; ASTM D573
Elongation at Break 350 %350 %Original; ASTM D412
 <= 175 %
@Temperature 100 °C,
Time 252000 sec
<= 175 %
@Temperature 212 °F,
Time 70.0 hour
Heat Aged; ASTM D573
 <= 262.5 %
@Temperature 100 °C,
Time 252000 sec
<= 262.5 %
@Temperature 212 °F,
Time 70.0 hour
A14 – Heat Resistance; ASTM D573
Compression Set  <= 25 %
@Temperature 70.0 °C,
Time 79200 sec
<= 25 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395 Method B
 <= 50 %
@Temperature 70.0 °C,
Time 79200 sec
<= 50 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395 S
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 116 °C240 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
 
Descriptive Properties
Hardness45-75Heat Aged, ASTM D573, 70 h @ 100°C
 55-65ASTM D2240
 70A14 – Heat Resistance, ASTM D573, 70 hours @ 100°C
Resistance to Ozone100C12, ASTM D1171

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBRPM042 / 315703

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.