MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Saint-Gobain Spectrosil® 2200 Optical Fused Quartz
Categories: Ceramic; Glass; Oxide; Silicon Oxide

Material Notes: Spectrosil® 2200 grade is an excimer laser grade developed for maximum transmission and prolonged life in microlithography and other critical deep UV applications using KrF (248 nm) and ArF (193 nm) excimer lasers.

Spectrosil® is a synthetic fused silica manufactured using a patented, environmentally friendly process that results in a virtually chlorine-free material of exceptional purity which is bubble-free and fluorescence-free. The 2000 series has excellent optical transmission from 180 nm in the deep UV through to 2000 nm in the IR Available in ingot, rod, tube, and components.

General properties of Fused Silica and Fused quartz: A very wide transmission range from UV to near IR; extremely high optical transmission, excellent resistance to high power laser energy, excellent homogeneity, high temperature resistance, very low thermal expansion (resistance to thermal shock), and chemical inertness. General uses for optical quartz are microlithography optical systems, optical fibers, photomasks, laser optics, LCD displays, light guides, optical, IR , and UV windows, spectrophotometer cells, slides, optical pyrometers, and lamp bodies/components.

Information provided by Saint-Gobain Quartz PLC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.21 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Knoop 820
Vickers Microhardness 1050 - 1350kg/m² Vickers DPH
Hardness, Mohs 7.0
Modulus of Elasticity 74.0 GPa
Flexural Strength 50.0 MPaBending Strength
Compressive Strength 1100 MPa
Poissons Ratio 0.17
Shear Modulus 31.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 2.00e+10 ohm-cm
@Temperature 800 °C
Dielectric Constant 3.78
@Frequency 100 - 2.50e+10 Hz
Dissipation Factor 0.000060
@Frequency 1e+9 Hz
 0.00075
@Frequency 1000 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 0.540 µm/m-°C
@Temperature 0.000 - 1000 °C
average
Specific Heat Capacity 0.750 J/g-°C
Thermal Conductivity 2.00 W/m-K
Maximum Service Temperature, Air 1050 °CNormal Conditions
 1350 °CExtended periods if cycles remain above 300°C
 1350 °C
 1650 °CQuick Immersion
Softening Point 1710 °CVaries with thermal history
Annealing Point 1100 °CVaries with thermal history
Strain Point 990 °CVaries with thermal history
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.457
@Wavelength 632.8 nm
nHe-Ne; Temperature Coefficient = 10.0 ppm/K
 1.4667
@Wavelength 435.83 nm
ng; Temperature Coefficient = 10.6 ppm/K
Transmission, Visible 95 %Including Fresnel reflection for 10 mm pathlength
UV Transmittance 95 %
@Wavelength <=200 nm,
Thickness 10.0 mm
Including Fresnel reflection for 10 mm path length.
 >= 99.5 %
@Thickness 10.0 mm,
Wavelength 193.4 nm
 >= 99.9 %
@Thickness 10.0 mm,
Wavelength 240 nm
 
Component Elements PropertiesOriginal ValueComments
SiO2 >= 99.999 %
 
Descriptive Properties
Bubble Class0per DIN 58927
Bubbles; Sum of CSA< 0.03 mm²/100 cm³
Inclusions0
Refractive Index Homogeneity< 10 x 10-6Up to 200 mm (ingot/blank)
 < 5 x 10-6Up to 100 mm (ingot/blank)
Residual Strain<5 nm/cm
Striae3per MIL-G-174A; Direction Free

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Saint-Gobain Spectrosil® 2000 Optical Fused Quartz
Corning Willow® Flexible Display Glass
Ohara BSM51Y i-Line Optical Glass
Schott N-F2 Glass
Schott N-LAF33 Glass

CSTGQZ04 / 2222

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.