MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Northstar Polymers MSS-A85BQ High Performance Polyurethane Cast Elastomer System 85A
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Liquid

Material Notes: This is a Ester/MDI base high-performance polyurethane casting system. This systems is recommended to applications in which the part requires high tensile strength, cut/tear resistance, dry-abrasion resistance, slow response speed, and low energy rebound/response. Ester base systems are generally less expensive than PTMEG base material. Possible applications for this material include skirting for conveyer belts, abrasion resistance liners and parts, and other specialty parts. Unlike conventional full-prepolymer systems, quasi system formulation improves processability, in-mold flow, and components mixing by use of low viscosity prepolymer. This results better physical properties of the products. Can be approved for FDA dry food contact.

Information provided by Northstar Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 85ASTM D2240
Tensile Strength 6200 psiASTM D412
Elongation at Break 800 %ASTM D412
100% Modulus 1.235 ksi
@Strain 100 %
ASTM D412
300% Modulus 2.91 ksi
@Strain 300 %
ASTM D412
Rebound 38 %Bashore Rebound; ASTM D2632
Tear Strength 475 pliSplit; ASTM D624
 720 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 30ASTM D4060
 
Processing PropertiesOriginal ValueComments
Processing Temperature 70.0 °FPrepolymer Temperature
 180 °FCuring Agent Temperature
Mold Temperature 180 °F
Cure Time 0.500 - 0.670 hour
@Temperature 82.2 °C
De-mold Time
 16.0 - 24.0 hour
@Temperature 82.2 °C
Complete Cure Cycle
Pot Life 2.50 - 3.00 min
Gel Time 4.00 min
 
Descriptive Properties
Curing AgentSBA-030
PrepolymerMSA-018
Weight Ratio1:1.636Prepolymer to Curing Agent Ratio

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Covestro Baydur® GS PUR Polyurethane
Covestro Baydur® GS PIR B Polyurethane
BCC Products BC 8990 Polyurethane Elastomer
BCC Products BC 8690E Polyurethane Elastomer
BASF Elastollan® S 95 A TPUR

PNORTH06 / 54841

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.