MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV 4145 D Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 4100 series are engineered materials designed primarily for demanding automotive and industrial applications. Available in both black and natural, this product is a low density, high hardness thermoplastic vulcanizate that exhibits excellent compression set, chemical resistance and high temperature performance. The material can be processed by injection molding, blow molding and extrusion for applications such as seals, gaskets, chemical resistant hose and tube, boots and bellows.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Alcohol Resistant; Chemical Resistant; Fatigue Resistant; Good Adhesion; Good Moldability; Good Processability; Good Surface Finish; Heat Aging Resistant; High Elasticity; High Hardness; High Melt Stability; Low Density; Low Specific Gravity; Medium Heat Resistant; Resilient

Uses: Appliance Components; Automotive Applications; Automotive Exterior Parts; Automotive Interior Parts; Automotive Under the Hood; Blow Molding Applications; Grommets; Hose; Plugs; Profiles; Rubber Replacement; Seals; Valves/Valve Parts; White Goods & Small Appliance

RoHS Compliance: RoHS Compliant

Automotive Specifications: CHRYSLER MS-AR-100 GCN Color: Black; CHRYSLER MS-AR-100 GCN Color: Natural; GM GMP.E/P.007 Color: Black; GM GMP.E/P.007 Color: Natural; GM GMW/15813 Type 10 Color: Black; GM GMW/15813 Type 10 Color: Natural

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.940 g/cc0.0340 lb/in³ISO 1183
Viscosity 440 cP
@Shear Rate 206 1/s,
Temperature 200 °C
440 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D  47
@Time 5.00 sec
47
@Time 0.00139 hour
Extruded; ISO 868
 51
@Time 5.00 sec
51
@Time 0.00139 hour
Injection Molded; ISO 868
Tensile Strength at Break 21.6 MPa3130 psiFlow; ISO 37
 23.1 MPa3350 psiAcross Flow; ISO 37
 19.6 MPa
@Treatment Temp. 150 °C,
Time 605000 sec
2850 psi
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
 21.2 MPa
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
3080 psi
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
Tensile Stress at Strain  13.0 MPa
@Strain 100 %
1890 psi
@Strain 100 %
Across Flow; ISO 37
 18.0 MPa
@Strain 100 %
2610 psi
@Strain 100 %
Flow; ISO 37
 15.0 MPa
@Strain 100 %,
Treatment Temp. 150 °C
2170 psi
@Strain 100 %,
Treatment Temp. 302 °F
Across Flow, Change in Air at 168 hr; ISO 188
 16.3 MPa
@Strain 100 %,
Treatment Temp. 135 °C
2360 psi
@Strain 100 %,
Treatment Temp. 275 °F
Across Flow, Change in Air at 1000 hr; ISO 188
Elongation at Break 420 %420 %Flow; ISO 37
 740 %740 %Across Flow; ISO 37
 592 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
592 %
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
 592 %
@Treatment Temp. 150 °C,
Time 605000 sec
592 %
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
Tear Strength 142 kN/m810 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set  55 %
@Temperature 22.8 °C,
Time 79200 sec
55 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 64 %
@Temperature 70.0 °C,
Time 79200 sec
64 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 85 %
@Temperature 125 °C,
Time 252000 sec
85 %
@Temperature 257 °F,
Time 70.0 hour
ISO 815
 
Processing PropertiesMetricEnglishComments
Processing Temperature 187 - 220 °C369 - 428 °FInjection
Rear Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Middle Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Front Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Nozzle Temperature 187 - 220 °C369 - 428 °FInjection
Zone 1 180 - 200 °C356 - 392 °FExtrusion
Zone 2 180 - 205 °C356 - 401 °FExtrusion
Zone 3 187 - 210 °C369 - 410 °FExtrusion
Zone 4 187 - 210 °C369 - 410 °FExtrusion
Die Temperature 195 - 215 °C383 - 419 °FExtrusion
Melt Temperature 195 - 215 °C383 - 419 °FExtrusion
Mold Temperature 10.0 - 55.0 °C50.0 - 131 °FInjection
Drying Temperature 82.2 °C180 °F
Dry Time 3.00 hour3.00 hour
Screw Speed 100 - 200 rpm100 - 200 rpmInjection
 
Descriptive Properties
AppearanceBlack
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Sarlink® TPV 4139D Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 6775N Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 6765N Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 4175 Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 4165 Thermoplastic Vulcanizate

PTEKNQ1155 / 237646

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.