MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Amodel® ET-1001 L Polyphthalamide (PPA) Resin, Dry as Molded  (discontinued **)
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), High Impact

Material Notes: AMODEL ET-1001 L resin is an impact modified polyphthalamide (PPA) with exceptional impact strength and practical toughness. AMODEL PPA resins offer high fatigue strength, and good chemical resistance combined with good mechanical property retention over a broad temperature/ humidity range.

Possible applications for AMODEL ET-1001 L resin include anti-friction and wear resistant components, and components of chemical and oil processing equipment, sporting goods, automobiles, household appliances, power tools, and safety equipment, where exceptional impact strength and high modulus are required.

AMODEL ET-1001 L resin contains a lubricant for easier processing with conventional equipment and methods.

Information provided by Solvay Advanced Polymers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.13 g/ccISO 1183A
 1.15 g/ccASTM D792
Moisture Absorption at Equilibrium 0.70 %24 hours; ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 55.0 MPaISO 527
 31.0 MPa
@Temperature 100 °C
ISO 527
Tensile Strength, Yield 58.0 MPaISO 527
 76.0 MPaASTM D638
 32.0 MPa
@Temperature 100 °C
ISO 527
Elongation at Break 15 %ISO 527
 30 %ASTM D638
 54.3 %
@Temperature 100 °C
ISO 527
Elongation at Yield 6.0 %ASTM D638
 6.0 %ISO 527
 3.1 %
@Temperature 100 °C
ISO 527
Tensile Modulus 2.30 GPaISO 527
 2.40 GPaASTM D638
 1.80 GPa
@Temperature 100 °C
ISO 527
Flexural Strength 66.0 MPaISO 178
 128 MPaASTM D790
 42.0 MPa
@Temperature 100 °C
ISO 178
Flexural Modulus 1.90 GPaISO 178
 2.60 GPaASTM D790
 1.30 GPa
@Temperature 100 °C
ISO 178
Poissons Ratio 0.35
Shear Modulus 0.852 - 0.889 GPaCalculated
Shear Strength 53.0 MPaASTM D732
Izod Impact, Notched 960 J/mASTM D256
Izod Impact, Notched (ISO) 80.0 kJ/m²ISO 180/1A
Izod Impact, Unnotched (ISO) NBISO 180/1U
Charpy Impact Unnotched NBISO 179/1eU
Charpy Impact, Notched NBISO 179/1eA
Dynatup @ -18°C 43.0 JEnergy at Maximum Load. Dry as molded. 23°C; D3763
 46.0 JEnergy at Maximum Load. Dry as molded. -23°C; D3763
 64.0 JTotal Energy. Dry as molded. 23°C; D3763
 66.0 JTotal Energy. Dry as molded. -23°C; D3763
Dynatup @ -18°C Max Load 1260 lb23°C; D3763
 1460 lb-23°C; D3763
 
Thermal PropertiesOriginal ValueComments
Melting Point 310 °CASTM D3418
 310 °CISO 11357-3
Deflection Temperature at 1.8 MPa (264 psi) 113 °CISO 75Af
 120 °CASTM D648

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Syensqo (Solvay Specialty Polymers) Amodel® ET-1001 HS Polyphthalamide (PPA) Resin, Dry As Molded
Syensqo (Solvay Specialty Polymers) Amodel® ET-1001 L Polyphthalamide (PPA) Resin, at 50% RH
Aluminum, Al
Syensqo (Solvay Specialty Polymers) Amodel® AT-5001 Polyphthalamide (PPA) Resin, at 50% RH
Syensqo (Solvay Specialty Polymers) Amodel® AT-5001 Polyphthalamide (PPA) Resin, Dry as Molded

PSOLVT74 / 21370

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.