MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Arkema Kynar® 710 Polyvinylidene Fluoride Homopolymer- Injection Molding
Categories: Polymer; Thermoplastic; Fluoropolymer; Polyvinylidene Fluoride (PVDF); Polyvinylidinefluoride (PVDF), Molded/Extruded

Material Notes: Characteristics: Natural resin - translucent, off-white hemispheres. HDP indicates higher color stability. High stability in harsh thermal, chemical and ultraviolet environments. High toughness and mechanical strength, low permeability, fire resistance, abrasion resistance; low-smoke emission; high purity

Applications:

  • Chemical processing – production, storage and transfer of corrosive fluids
  • Electronics – protective sheathing, plenum and wiring insulation
  • Semi-conductor industry
  • Food stuff and Healthcare industries
  • Transportation – fuel line and pipe, thermoformed body components

Listed properties are typical for 700 series.

Information provided by Arkema Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.77 - 1.79 g/ccASTM D792
Density 1.78 g/ccISO 1183
Water Absorption 0.010 - 0.030 %ASTM D570
 0.030 %Dry; Sim. to ISO 62
Viscosity 400000 - 800000 cP
@Shear Rate 100 1/s,
Temperature 230 °C
Melt; ASTM D3835
Linear Mold Shrinkage, Flow 0.020 cm/cmDry; ISO 294-4, 2577
 0.020 cm/cm
Melt Flow 20 g/10 min
@Load 5.00 kg,
Temperature 230 °C
cm³/10 min Volumetric Rate; ISO 1133
 19 - 35 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 76 - 80ASTM D2240
Tensile Strength at Break 34.5 - 55.2 MPaASTM D638
Tensile Strength, Yield 44.8 - 55.2 MPaASTM D638
 54.0 MPaDry; ISO 527-1/-2
Elongation at Break >= 50 %Dry; ISO 527-1/-2
 20 - 100 %ASTM D638
Elongation at Yield 5.0 - 10 %ASTM D638
 9.0 %Dry; ISO 527-1/-2
Tensile Modulus 1380 - 2310 MPaASTM D638
 2300 MPaDry; ISO 527-1/-2
Flexural Strength 58.6 - 75.8 MPa
@Strain 5.0 %
ASTM D790
Flexural Modulus 1380 - 2310 MPaASTM D790
Compressive Strength 68.9 - 103 MPaASTM D695
Izod Impact, Notched 80.1 - 214 J/mASTM D256
Izod Impact, Unnotched 1070 - 4270 J/mASTM D256
Charpy Impact Unnotched 192 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eU
 208 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eA
 8.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eA
Coefficient of Friction, Dynamic 0.14vs. steel; ASTM D1894
Coefficient of Friction, Static 0.20vs. steel; ASTM D1894
Taber Abrasion, mg/1000 Cycles 5.0 - 9.0CS 17 1000g:pad; ASTM-G195-13A
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 2.00e+14 ohm-cm65% R.H; ASTM D257
 2.00e+14 ohm-cmDry; IEC 60093
Dielectric Constant 6.0
@Frequency 1e+6 Hz
Dry; IEC 60250
 4.5 - 9.5
@Frequency 1000 Hz
ASTM D150
 9.0
@Frequency 100 Hz
Dry; IEC 60250
Dielectric Strength >= 1.70 kV/mm
Dissipation Factor 0.035
@Frequency 100 Hz
Dry; IEC 60250
 0.010 - 0.21
@Frequency 100000 Hz
ASTM D150
 0.206
@Frequency 1e+6 Hz
Dry; IEC 60250
 
Thermal PropertiesOriginal ValueComments
CTE, linear 119 - 144 µm/m-°CASTM D696
CTE, linear, Parallel to Flow 150 µm/m-°CDry; ISO 11359-1/-2
Specific Heat Capacity 0.665 - 0.958 J/g-°CDSC
Thermal Conductivity 0.170 - 0.190 W/m-KASTM D433
Melting Point 168 °C10°C/min; Dry; ISO 11357-1/-3
 165 - 172 °CASTM D3418
Maximum Service Temperature, Air 150 °CUL RTI
Deflection Temperature at 0.46 MPa (66 psi) 130 °CDry; ISO 75-1/-2
 125 - 140 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 105 - 115 °CASTM D648
 110 °CDry; ISO 75-1/-2
Vicat Softening Point 140 °C50°C/h 50N; Dry; ISO 306
Glass Transition Temp, Tg -40.0 °C10°C/min; Dry; ISO 11357-1/-2
 -40.6 - -38.3 °CASTM D7028
Decomposition Temperature 375 °C1% wt. loss, TGA, in air
 410 °C1% wt. loss, TGA, in nitrogen
UL RTI, Electrical 150 °CUL 746B
UL RTI, Mechanical without Impact 150 °CUL 746B
Flammability, UL94 V-0
@Thickness 0.800 mm
IEC 60695-11-10
 V-0
@Thickness 1.60 mm
Yellow Card Available; Dry; IEC 60695-11-10
Oxygen Index 43 %Dry; ISO 4589-1/-2
 44 %ASTM D2863
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.42sodium D line; ASTM D542
 
Processing PropertiesOriginal ValueComments
Melt Temperature 200 °CInjection Molding; ISO 294
Mold Temperature 90.0 °CInjection Molding; ISO 10724
Injection Velocity 10.0 mm/secInjection Molding; ISO 294
Hold Pressure 13.0 MPaInjection Molding; ISO 294
 
Descriptive Properties
Form as DeliveredPellets
Heat StabilizedYes
Light StabilizedYes
Moisture SensitiveNo
Processing MethodsFilm Extrusion
 Injection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Saint-Gobain Norton® PVDF Fluoropolymer Film
Arkema Kynar® 720 Polyvinylidene Fluoride Homopolymer- Injection Molding and Extrusion
Arkema KYNAR® 370 Polyvinylidene Fluoride (PVDF) Homopolymer - Injection Molding
Arkema KYNAR® 9000 HD Polyvinylidene Fluoride - Injection Molding
AGC Fluon® PTFE

PARKG904 / 144529

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.