MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
DSM Arnite® T08 200 (extrusion) T08 200 PBT (European and Asian Grade)  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Unreinforced, Molded

Material Notes: Arnite resins are engineered to provide specific performance in applications where DSM technology can offer value.

Arnite Molding resins:

  • Standard Unfilled and Reinforced materials
  • High modulus Flame retardant grades
  • Easy molding FR grades for connectors
  • Toughened unfilled materials for durability
  • High modulus, tight specification for critical auto components
  • Toughened reinforced resins
  • Low outgassing grades for reflector surfaces

Arnite extrusion resins: Specialized materials for specific uses

  • PET for medical applications
  • Loose buffer Optical fiber tubing
  • PET for stock shapes

Applications

  • Automotive:Connectors, sensors and E&E parts, Exterior fittings, Gear housings and motors, Brake valve bodies
  • Electrical & Electronic: Telecoms and IT connectors, Bobbins, Low voltage Power distribution, E-motor components, Lightings and Lamp fittings
  • Consumer Durables: Small Appliances
  • Other: Optical fiber tubing

Information provided by DSM.

Artnite is a former DSM Engineering Plastics product line now with Envalior, although this specific product was discontinued prior to that transaction

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.30 g/ccISO 1183
Water Absorption 0.45 %Sim. to ISO 62
Moisture Absorption at Equilibrium 0.18 %Humidity Absorption; Sim. to ISO 62
Melt Flow 13 g/10 min
@Load 2.16 kg,
Temperature 250 °C
Calculated from Volume Flow Rate of 10 cm3/10min.; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 55.0 MPaISO 527-1/-2
Elongation at Break >= 50 %ISO 527-1/-2
Elongation at Yield 3.5 %ISO 527-1/-2
Tensile Modulus 2.80 GPaISO 527-1/-2
Charpy Impact Unnotched NB
@Temperature -30.0 °C
ISO 179/1eU
 NB
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 0.600 J/cm²
@Temperature -30.0 °C
ISO 179/1eA
 0.600 J/cm²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmIEC 60093
Dielectric Constant 3.2
@Frequency 1e+6 Hz
IEC 60250
 3.5
@Frequency 100 Hz
IEC 60250
Dielectric Strength 27.0 kV/mmIEC 60243-1
Dissipation Factor 0.0020
@Frequency 100 Hz
IEC 60250
 0.020
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 VIEC 60112
 >= 600 VPLC 0; UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 70.0 µm/m-°C
@Temperature 20.0 °C
ISO 11359-1/-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature 20.0 °C
ISO 11359-1/-2
Melting Point 225 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 170 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °CISO 75-1/-2
UL RTI, Electrical 130 °C
@Thickness 1.50 mm
UL746B
 130 °C
@Thickness 0.750 mm
UL746B
UL RTI, Mechanical with Impact 95.0 °C
@Thickness 0.750 mm
UL746B
 110 °C
@Thickness 1.50 mm
UL746B
UL RTI, Mechanical without Impact 125 °C
@Thickness 0.750 mm
UL746B
 130 °C
@Thickness 1.50 mm
UL746B
Flammability, UL94 HB
@Thickness 1.60 mm
IEC 60695-11-10
 HB
@Thickness 0.750 mm
IEC 60695-11-10
 
Descriptive Properties
Injection MoldingYes
Other ExtrusionYes
Without FillersYes

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Celanex® 3300 PBT, 30% Glass Reinforced
BorsodChem ONGRO CPE 4002 N Chlorinated Polyethylene

PDSMEU348 / 31295

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.