MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Stratasys® Antero™ 800NA PEKK-based FDM 3D Printing Polymer
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polyketone; PEKK, Unreinforced

Material Notes: Antero™ 800NA is a PEKK-based FDM® thermoplastic with excellent mechanical properties that include high strength, high heat resistance, toughness and wear-resistance. These qualities make it a lighter alternative to aluminum and steel in certain use cases. Chemical resistance and minimal outgassing provide suitability for aerospace applications where prototypes and parts are exposed to jet fuel, oil and hydraulic fluid. Other uses include industrial applications where high-strength and chemical resistance are needed. 3D printing with Antero 800NA FDM filament avoids the waste associated with subtractive manufacturing of high-cost bulk PEKK material.

Information provided by Stratasys.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.28 g/cc1.28 g/ccXY, XZ/ZX Orientations; ASTM D257
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 45.0 MPa6530 psiZX Orientation, Fortus 450mc w/T20D tip; ASTM D638
 55.0 MPa7980 psiZX Orientation, F900 w/T20D tip; ASTM D638
 70.0 MPa10200 psiXZ Orientation, F900 w/T20D tip; ASTM D638
 70.0 MPa10200 psiXZ Orientation, Fortus 450mc w/T20D tip; ASTM D638
Tensile Strength, Yield 90.0 MPa13100 psiXZ Orientation, F900 w/T20D tip; ASTM D638
 93.0 MPa13500 psiXZ Orientation, Fortus 450mc w/T20D tip; ASTM D638
Elongation at Break 1.2 %1.2 %ZX Orientation, Fortus 450mc w/T20D tip; ASTM D638
 1.9 %1.9 %ZX Orientation, F900 w/T20D tip; ASTM D638
 6.0 %6.0 %XZ Orientation, F900 w/T20D tip; ASTM D638
 6.0 %6.0 %XZ Orientation, Fortus 450mc w/T20D tip; ASTM D638
Elongation at Yield 4.3 %4.3 %XZ Orientation, F900 w/T20D tip; ASTM D638
 4.3 %4.3 %XZ Orientation, Fortus 450mc w/T20D tip; ASTM D638
Modulus of Elasticity 2.90 GPa421 ksiXZ Orientation, F900 w/T20D tip; ASTM D638
 2.90 GPa421 ksiZX Orientation, F900 w/T20D tip; ASTM D638
 3.10 GPa450 ksiXZ Orientation, Fortus 450mc w/T20D tip; ASTM D638
 3.50 GPa508 ksiZX Orientation, Fortus 450mc w/T20D tip; ASTM D638
Flexural Strength 65.0 MPa9430 psiZX Orientation, Fortus 450mc w/T20D tip; ASTM D790, Procedure A
 90.0 MPa13100 psiXZ Orientation, F900 w/T20D tip; ASTM D790, Procedure A
 140 MPa
@Strain 5.0 %
20300 psi
@Strain 5.0 %
XZ Orientation, Fortus 450mc w/T20D tip; ASTM D790, Procedure A
 140 MPa
@Strain 5.0 %
20300 psi
@Strain 5.0 %
ZX Orientation, F900 w/T20D tip; ASTM D790, Procedure A
Flexural Modulus 2.70 GPa392 ksiZX Orientation, F900 w/T20D tip; ASTM D790, Procedure A
 2.70 GPa392 ksiZX Orientation, Fortus 450mc w/T20D tip; ASTM D790, Procedure A
 3.10 GPa450 ksiXZ Orientation, F900 w/T20D tip; ASTM D790, Procedure A
 3.10 GPa450 ksiXZ Orientation, Fortus 450mc w/T20D tip; ASTM D790, Procedure A
Flexural Strain at Break 2.4 %2.4 %ZX Orientation, Fortus 450mc w/T20D tip; ASTM D790, Procedure A
 3.3 %3.3 %ZX Orientation, F900 w/T20D tip; ASTM D790, Procedure A
Compressive Yield Strength 93.0 MPa13500 psiZX Orientation, F900 w/T20D tip; ASTM D695
 97.0 MPa14100 psiXZ Orientation, F900 w/T20D tip; ASTM D695
 100 MPa14500 psiXZ Orientation, Fortus 450mc w/T20D tip; ASTM D695
 101 MPa14600 psiZX Orientation, Fortus 450mc w/T20D tip; ASTM D695
Compressive Modulus 2.18 GPa316 ksiZX Orientation, F900 w/T20D tip; ASTM D695
 2.30 GPa334 ksiZX Orientation, Fortus 450mc w/T20D tip; ASTM D695
 2.35 GPa341 ksiXZ Orientation, F900 w/T20D tip; ASTM D695
 2.45 GPa355 ksiXZ Orientation, Fortus 450mc w/T20D tip; ASTM D695
Izod Impact, Notched 0.300 J/cm0.562 ft-lb/inZX Orientation, F900 w/T20D tip; ASTM D256, ASTM D4812
 0.300 J/cm0.562 ft-lb/inZX Orientation, Fortus 450mc w/T20D tip; ASTM D256, ASTM D4812
 0.350 J/cm0.656 ft-lb/inXZ Orientation, Fortus 450mc w/T20D tip; ASTM D256, ASTM D4812
 0.450 J/cm0.843 ft-lb/inXZ Orientation, F900 w/T20D tip; ASTM D256, ASTM D4812
Izod Impact, Unnotched 0.750 J/cm1.41 ft-lb/inZX Orientation, Fortus 450mc w/T20D tip; ASTM D256, ASTM D4812
 1.50 J/cm2.81 ft-lb/inZX Orientation, F900 w/T20D tip; ASTM D256, ASTM D4812
 15.5 J/cm29.0 ft-lb/inXZ Orientation, F900 w/T20D tip; ASTM D256, ASTM D4812
 18.2 J/cm34.1 ft-lb/inXZ Orientation, Fortus 450mc w/T20D tip; ASTM D256, ASTM D4812
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 5.50e+14 ohm-cm>= 5.50e+14 ohm-cmASTM D257
Dielectric Constant 3.3
@Frequency 1000 Hz
3.3
@Frequency 1000 Hz
XY, XZ/ZX Orientations; ASTM D150
Dissipation Factor 0.0030
@Frequency 1000 Hz
0.0030
@Frequency 1000 Hz
XY, XZ/ZX Orientations; ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear  35.0 µm/m-°C
@Temperature 40.0 - 140 °C
19.4 µin/in-°F
@Temperature 104 - 284 °F
XY Orientation; ASTM E831
 50.0 µm/m-°C
@Temperature 40.0 - 140 °C
27.8 µin/in-°F
@Temperature 104 - 284 °F
XZ/ZX Orientation; ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 150 °C302 °FXY, XZ/ZX Orientations; ASTM D648 Method B
Deflection Temperature at 1.8 MPa (264 psi) 147 °C297 °FXY, XZ/ZX Orientations; ASTM D648 Method B
Glass Transition Temp, Tg 149 °C300 °FInflection Point, XY, XZ/ZX; ASTM D7426

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSTRAS905 / 255800

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.