MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Evonik VESTAKEEP® i2 G PEEK
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Unreinforced

Material Notes: VESTAKEEP® i2 G is a natural colored, standard viscosity polyether ether ketone (PEEK) that is especially designed for long term implantable medical devices. This grade is often used for injection molding processing technologies due to its good flowability.
Dry properties listed below
Industrial Sector: Medical Devices
Processing: Injection molding , Extrusion
Delivery form: Pellets, Granules
Optics: Opaque
Conformity: Biocompatibility, Medical application
Additives: Unfilled
Special Characteristics: Semi-crystalline
Regulatory: US Pharmacopeia Class VI conformity
Color: Natural color
Chemical Resistance: Acid resistance, Alkali resistance, Solvent resistance, Grease resistance, Hydrolytically stable, Oil resistance, Oxidation resistance, General chemical resistance

Information provided by Evonik.

Vendors: Ensinger TECAPEEK™ shapes are manufactured exclusively with Victrex™ PEEK polymer. The Ensinger process and Victrex resins ensure reliability, consistency, dimensional stability, and high temperature mechanical performance.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.30 g/ccISO 1183
Water Absorption 0.400 %Sim to ISO 62
Moisture Absorption 0.120 %Sim to ISO 62
Linear Mold Shrinkage, Flow 0.0110 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0110 cm/cmISO 294-4, 2577
Melt Flow 68.0 g/10 min
@Load 5.00 kg,
Temperature 380 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 74.0 MPaISO 527
Tensile Strength 98.0 MPaISO 527
Tensile Strength, Yield 98.0 MPaISO 527
Elongation at Break 20.0 %Nominal; ISO 527
Elongation at Yield 5.00 %ISO 527
Tensile Modulus 3700 MPaISO 527
Flexural Strength 117 MPaISO 178
Flexural Modulus 3600 MPaISO 178
Charpy Impact Unnotched NB
@Temperature 23.0 °C
ISO 179/1eU
 NB
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 6.00 kJ/m²
@Temperature 23.0 °C
Type of failure: C; ISO 179/1eA
 6.00 kJ/m²
@Temperature -30.0 °C
Type of failure: C; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+13 ohm-cm?V; IEC 62631-3-1
Dielectric Constant 2.80
@Frequency 100 Hz
IEC 62631-2-1
 2.80
@Frequency 1.00e+6 Hz
IEC 62631-2-1
Dielectric Strength 16.0 kV/mmAC, S20/P50; Sim to IEC 60243-1
Dissipation Factor 0.00500
@Frequency 1.00e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 200 Vtest solution A, 50 drops value; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 60.0 µm/m-°C
@Temperature 25.0 - 55.0 °C
ISO 11359-1/-2
Melting Point 342 °CISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 205 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 150 °CISO 75-1/-2
Vicat Softening Point 310 °C
@Load 5.10 kg
50 K/h; ISO 306
 335 °C
@Load 1.02 kg
50 K/h; ISO 306
Glass Transition Temp, Tg 150 °CISO 11357-1/-2
Flammability, UL94 V-0
@Thickness 3.20 mm
IEC 60695-11-10
Oxygen Index 38.0 %ISO 4589-1/-2
 38.0 %ASTM D2863
 
Processing PropertiesOriginal ValueComments
Melt Temperature 360 °C
 380 °CInjection Molding; ISO 294
Mold Temperature 180 °CInjection Molding; ISO 294
 180 °C
Injection Velocity 200 mm/secInjection Molding; ISO 294
 
Descriptive Properties
ColorNatural Color

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PEVONIK7861 / 324993

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.