MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Fujipoly Industries Sarcon® 30GHR Thin-Film GHR
Categories: Polymer; Film; Thermoset; Silicone

Material Notes: Sarcon HR is Fujipolys originally developed High Heat Conductive Silicone Rubber. Fine, high heat conductive ceramic particles are mixed with insulative silicone rubber.

Sarcon GHR is a composite of Heat Conductive Silicone Rubber and fiberglass.

Information provided by Fujipoly Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 95ASTM D2240
 9560°C for 500 hrs; ASTM D2240
 96150°C for 1,000 hrs; ASTM D2240
 96200°C for 1,000 hrs; ASTM D2240
Tensile Strength, Yield 24.0 MPa200°C for 1,000 hrs
 26.6 MPaASTM D1458
 31.67 MPa150°C for 1,000 hrs; ASTM D1458
Elongation at Yield <= 2.0 %ASTM D1458
 <= 2.0 %150°C for 1,000 hrs; ASTM D1458
 <= 2.0 %200°C for 1,000 hrs; ASTM D1458
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 3.90e+9 ohm-cm60°C for 500 hrs
 1.00e+15 ohm-cm
 3.90e+15 ohm-cm150°C for 1,000 hrs
 1.00e+16 ohm-cm200°C for 1,000 hrs
Dielectric Constant 3.1
@Frequency 50 Hz
After 1000 hrs at 150°C
 3.1
@Frequency 1e+6 Hz
After 1000 hrs at 150°C
 3.1
@Frequency 1000 Hz
After 1000 hrs at 150°C
 3.5
@Frequency 1000 Hz
After 1000 hrs at 200°C
 3.5
@Frequency 1e+6 Hz
After 1000 hrs at 200°C
 3.5
@Frequency 50 Hz
After 1000 hrs at 200°C
 3.9
@Frequency 50 Hz
 3.9
@Frequency 1000 Hz
 3.9
@Frequency 1e+6 Hz
 4.5
@Frequency 1e+6 Hz
After 500 hrs at 60°C
 4.7
@Frequency 1000 Hz
After 500 hrs at 60°C
 5.0
@Frequency 50 Hz
After 500 hrs at 60°C
Dielectric Strength 5.70 kV/mm200°C for 1,000 hrs
 7.00 kV/mm60°C for 500 hrs
 7.00 kV/mm150°C for 1,000 hrs
 9.00 kV/mmAC 60 Hz
Dielectric Breakdown 8000 VWithstand Voltage [V/min]; AC 60 Hz
Dissipation Factor 0.0010
@Frequency 1000 Hz
After 1000 hrs at 200°C
 0.0020
@Frequency 50 Hz
After 1000 hrs at 200°C
 0.0020
@Frequency 50 Hz
After 1000 hrs at 150°C
 0.0020
@Frequency 1000 Hz
After 1000 hrs at 150°C
 0.0030
@Frequency 1e+6 Hz
After 1000 hrs at 200°C
 0.0030
@Frequency 1000 Hz
 0.0040
@Frequency 1e+6 Hz
 0.0040
@Frequency 1e+6 Hz
After 1000 hrs at 150°C
 0.0060
@Frequency 50 Hz
 0.0080
@Frequency 1e+6 Hz
After 500 hrs at 60°C
 0.020
@Frequency 1000 Hz
After 500 hrs at 60°C
 0.069
@Frequency 50 Hz
After 500 hrs at 60°C
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 182 °C
Minimum Service Temperature, Air -60.0 °C
Flammability, UL94 V-0
 
Descriptive Properties
ColorBrown
Thermal Impedance0.61°C/WFTM P-3010; ASTM D5470
Thermal Impedance AD Type0.72°C/WFTM P-3010; ASTM D5470

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Saxonburg Ceramics S-405 Cordierite
Sapco C 221 Steatite
Sapco C 220 Steatite
S-2 Glass® Fiber
Goodfellow Shapal™-M soft Aluminum Nitride (AlN) - Machinable

PFUJIP34 / 39167

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.