MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Poly Alloy VeryGreen™ VG7263 PLA
Categories: Polymer; Thermoplastic; Polylactic Acid (PLA) Biopolymer

Material Notes: VeryGreen™ VG7263 resin is a PLA compound for injection molding process. With high impact property, VG7263 can be used on general purpose applications. The composition of VG7263 complies with the requirements for use in contact with food of European Commission Regulation (EU) No 10/2011.

Information provided by Poly Alloy Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.27 g/cc1.27 g/ccASTM D792
Melt Flow 4.0 g/10 min
@Load 5.00 kg,
Temperature 210 °C
4.0 g/10 min
@Load 11.0 lb,
Temperature 410 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8282ASTM D2240
Tensile Strength 47.1 MPa6830 psiASTM D638
Elongation at Break 15 %15 %ASTM D638
Tensile Modulus 2.45 GPa356 ksiASTM D638
Flexural Strength 78.6 MPa11400 psiASTM D790
Flexural Modulus 3.92 GPa569 ksiASTM D790
Izod Impact, Notched  0.490 J/cm
@Temperature -30.0 °C
0.918 ft-lb/in
@Temperature -22.0 °F
ASTM D256
 1.77 J/cm
@Temperature 23.0 °C
3.31 ft-lb/in
@Temperature 73.4 °F
ASTM D256
Izod Impact, Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ASTM D256
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 90.0 °C194 °FASTM D648
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 175 - 185 °C347 - 365 °F
Middle Barrel Temperature 175 - 185 °C347 - 365 °F
Front Barrel Temperature 175 - 185 °C347 - 365 °F
Nozzle Temperature 175 - 185 °C347 - 365 °F
Mold Temperature 80.0 - 90.0 °C176 - 194 °F
Drying Temperature >= 70.0 °C>= 158 °F
Dry Time 4.00 hour4.00 hour
Dew Point <= -40.0 °C<= -40.0 °F
Shelf Life 24.0 Month24.0 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPALLOY124 / 278403

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.