MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Röchling Polystone® Marine-Tec lite PE-UHMW
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); UHMW PE (Ultra High Molecular Weight PE)

Material Notes: Product characteristics:
  • UV-stabilized and colorfast
  • Seawater resistant
  • Resistant against scratches
Product applications:
  • Boat building

Information provided by Röchling.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.800 g/cc0.0289 lb/in³DIN EN ISO 1183-1
Water Absorption <= 0.010 %<= 0.010 %DIN EN ISO 62
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6262DIN EN ISO 868
Tensile Strength, Yield 15.0 MPa2180 psiDIN EN ISO 527
Elongation at Break >= 25 %>= 25 %DIN EN ISO 527
Modulus of Elasticity 0.650 GPa94.3 ksiDIN EN ISO 527
Izod Impact, Notched (ISO) 8.00 kJ/m²3.81 ft-lb/in²DIN EN ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+14 ohm-cm>= 1.00e+14 ohm-cmDIN EN 62631-3-1
Surface Resistance >= 1.00e+14 ohm>= 1.00e+14 ohmDIN EN 62631-3-2
Dielectric Constant 2.52.5IEC 60250
Dielectric Strength 30.0 kV/mm762 kV/inIEC 60243
Dissipation Factor 0.00040
@Frequency 1e+6 Hz
0.00040
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 150 - 230 µm/m-°C83.3 - 128 µin/in-°FDIN 53752
Specific Heat Capacity 1.90 J/g-°C0.454 BTU/lb-°FDIN 52612
Thermal Conductivity 0.300 W/m-K2.08 BTU-in/hr-ft²-°FDIN 52612-1
Melting Point 135 °C275 °FISO 11357-3
Maximum Service Temperature, Air 80.0 °C176 °Flong term
 100 °C212 °Fshort term
Vicat Softening Point 67.0 °C153 °FDIN EN ISO 306, Vicat B
Minimum Service Temperature, Air -30.0 °C-22.0 °F
Flammability, UL94  HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 HB
@Thickness 6.00 mm
HB
@Thickness 0.236 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Coastal Enterprises Plus™ PBHT-40 High Density Urethane Foam
Rogers Corporation Poron® 4701-50 Supported Urethane Foam, Firm, PET Supported
Röchling Polystone® M XL Cross linked UHMW-PE
Overview of materials for High Density Polyethylene (HDPE), Ultra High Molecular Weight
Mitsubishi Chemical Advanced Materials TIVAR™ 1000 Virgin UHMW-PE, (Natural & Colors except Black)

PROCH9241 / 232944

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.