MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Titanium Ti-5-5-2-3 (Ti-5Mo-5V-2Cr-3Al), 60 mm Bar, Aged
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Relative to Ti-10V-2Fe-3Al. Characterized by cold formable and weldable high strength Ti alloy, in high area reduction and high fracture toughness KIC.

Applications:

  • Bars for deep well strings in the petroleum industry
  • Rods diameter 8-20 mm for high strength bolts
  • Near net shape forging application
  • Thick wall vessel
  • Ultra high velocity centrifugal rotor

Data provided by MarkeTech International

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 4.80 g/cc0.173 lb/in³estimated by MatWeb
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1300 MPa189000 psiAged Condition II
 1350 MPa196000 psiAged Condition I
Tensile Strength, Yield  1220 MPa
@Strain 0.2 %
177000 psi
@Strain 0.2 %
Aged Condition II
 1270 MPa
@Strain 0.2 %
184000 psi
@Strain 0.2 %
Aged Condition I
Elongation at Break 9.8 %9.8 %Aged Condition II
 10 %10 %Aged Condition I
Reduction of Area 22 %22 %Aged Condition I
 23 %23 %Aged Condition II
Modulus of Elasticity 113 GPa16400 ksiAged Condition II
 116 GPa16800 ksiAged Condition I
Fracture Toughness 57.3 MPa-m½52.1 ksi-in½Aged Condition I; KIC
 67.9 MPa-m½61.8 ksi-in½Aged Condition II; KIC
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 3.0 %3.0 %
Chromium, Cr 2.0 %2.0 %
Molybdenum, Mo 5.0 %5.0 %
Titanium, Ti 85 %85 %
Vanadium, V 5.0 %5.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-5-5-2-3 (Ti-5Mo-5V-2Cr-3Al), 12 mm Rod, Aged
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 760°C, Aged 385°C
Titanium Beta III (Ti-11.5Mo-6Zr-4.5Sn; Grade 10), ST 720°C, Aged 550°C
Titanium Beta III (Ti-11.5Mo-6Zr-4.5Sn; Grade 10), ST 775°C, Aged 495°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) Solution Treated 850°C (1560°F)

MTB026B / 14151

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.