MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
BASF Ultramid® 8231G HS 14% Glass Filled PA6 (Dry)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 10% Glass Fiber Filled

Material Notes: Ultramid 8231G HS is a heat stabilized, 14% glass fiber reinforced nylon 6 injection molding compound. It is also available in non-heat stabilized (Ultramid 8231) and/or pigmented versions. The glass fiber reinforcement enhances performance such as strength, stiffness and heat deflection temperature. The heat stabilizer system extends the properties at elevated temperatures. It also has excellent chemical resistance to greases, oils and hydrocarbons. njection molding compound possessing a balance of engineering properties combined with excellent processability and surface aesthetics.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.23 g/ccISO 1183
Melt Density 1.067 g/cc
@Temperature >=220 °C
ISO 1183
Water Absorption 1.4 %24 hour; ISO Test
 8.1 %ISO 62
Moisture Absorption at Equilibrium 2.3 %23°C/50% R.H.; ISO 62
Viscosity Measurement 50Formic Acid
Linear Mold Shrinkage 0.0050 cm/cmASTM Data; MD
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 121ASTM Test
Tensile Strength at Break 140 MPa0.2 in/min; ASTM Test
 50.0 MPa
@Temperature 120 °C
ISO Data
 50.0 MPa
@Temperature 120 °C
ASTM Test
 60.0 MPa
@Temperature 80.0 °C
ASTM Test
 60.0 MPa
@Temperature 80.0 °C
ISO Data
 160 MPa
@Temperature -40.0 °C
ASTM Test
 160 MPa
@Temperature -40.0 °C
ISO Data
Tensile Strength, Ultimate 140 MPa5mm/min; ISO 527
Elongation at Break 4.0 %5mm/min; ISO 527
 4.0 %0.2 in/min; ASTM Test
 3.0 %
@Temperature -40.0 °C
ASTM Test
 3.0 %
@Temperature -40.0 °C
ISO Data
 7.0 %
@Temperature 120 °C
ISO Data
 7.0 %
@Temperature 120 °C
ASTM Test
 8.0 %
@Temperature 80.0 °C
ASTM Test
 8.0 %
@Temperature 80.0 °C
ISO Data
Tensile Modulus 5960 MPa1mm/min; ISO 527
 2090 MPa
@Temperature 120 °C
ISO Data
 2470 MPa
@Temperature 80.0 °C
ISO Data
 5950 MPa
@Temperature -40.0 °C
ISO Data
Flexural Strength 160 MPaISO Data
 172 MPaASTM Test
 76.0 MPa
@Temperature 120 °C
ASTM Test
 90.0 MPa
@Temperature 93.0 °C
ASTM Test
 110 MPa
@Temperature 65.0 °C
ASTM Test
 214 MPa
@Temperature -40.0 °C
ASTM Test
Flexural Modulus 4770 MPaISO Data
 5310 MPaASTM Test
 1930 MPa
@Temperature 120 °C
ASTM Test
 2400 MPa
@Temperature 65.0 °C
ASTM Test
Izod Impact, Notched 0.590 J/cm
@Thickness 3.17 mm
ASTM Test
Izod Impact, Notched (ISO) 5.00 kJ/m²ISO Test
Charpy Impact Unnotched 4.00 J/cm²ISO 179
Charpy Impact, Notched 0.650 J/cm²ISO 179
 0.550 J/cm²
@Temperature -30.0 °C
ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+13 ohm-cmIEC 60093
Dielectric Constant 3.4
@Frequency 1e+6 Hz
IEC 60250
 3.6
@Frequency 100 Hz
IEC 60250
 3.7
@Frequency 1e+6 Hz
ASTM Data
 4.0
@Frequency 1e+9 Hz
ASTM Data
Dielectric Strength 40.0 kV/mmIEC 60243-1
Dissipation Factor 0.010
@Frequency 1e+9 Hz
ASTM Data
 0.010
@Frequency 1e+6 Hz
ASTM Data
 0.010
@Frequency 100 Hz
IEC 60250
 0.020
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesOriginal ValueComments
CTE, linear 50.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
ASTM Test
CTE, linear, Parallel to Flow 39.0 µm/m-°CISO 11359
CTE, linear, Transverse to Flow 78.0 µm/m-°CISO 11359
Specific Heat Capacity 2.728 J/g-°CMelt
Thermal Conductivity 0.230 W/m-KMelt
Melting Point 220 °C10 K/min
 220 °CASTM Test
Deflection Temperature at 0.46 MPa (66 psi) 217 °CISO 75
Deflection Temperature at 1.8 MPa (264 psi) 195 °CISO 75
 200 °CASTM Test
Flammability, UL94 HB
@Thickness 0.750 mm
 HB
@Thickness 3.00 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 275 °CInjection molding
Mold Temperature 95.0 °CInjection molding
 
Descriptive Properties
ColorNatural
Commercial StatusActive America
FormPellets
Impact ModifiedNo
Primary Processing TechniqueInjection Molding
ProcessingInjection Molding
Special characteristicHeat stabilized or stable to heat
UL.UL-CYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® 8231G HS 14% Glass Filled PA6 (Conditioned)
Custom Resins Nylene® 434 Un-reinforced Nylon 6
BASF Capron® 8231G 14% Glass-Filled Nylon 6 (Dry)
Envalior Akulon® K224-HG6 PA6-GF30, Dry, 30% Glass Filled, Heat Stabilized
BASF Ultramid® B3EG3 15% Glass Filled PA6 (Conditioned)

PBASF9153 / 84917

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.