MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

BASF Ultramid® B3S HP PA6 (Dry)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: Ultramid B3S HP is a easy flowing, finely crystalline, injection molding PA6 for fast processing

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.13 g/cc0.0408 lb/in³ISO 1183
Water Absorption 9.0 - 10 %9.0 - 10 %ISO 62
Moisture Absorption at Equilibrium 2.6 - 3.4 %2.6 - 3.4 %23°C/50% R.H.; ISO 62
Viscosity Number 145 cm³/g1.45 dl/gISO 307
Linear Mold Shrinkage 0.0050 cm/cm0.0050 in/in
Melt Flow 198 g/10 min
@Load 5.00 kg,
Temperature 275 °C
198 g/10 min
@Load 11.0 lb,
Temperature 527 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength  10.0 MPa
@Strain 1 %,
Temperature 100 °C
1450 psi
@Strain 1 %,
Temperature 212 °F
ISO 527
 18.0 MPa
@Strain 3 %,
Temperature 100 °C
2610 psi
@Strain 3 %,
Temperature 212 °F
ISO 527
 20.0 MPa
@Strain 1 %,
Temperature 60.0 °C
2900 psi
@Strain 1 %,
Temperature 140 °F
ISO 527
 30.0 MPa
@Strain 1 %,
Temperature 23.0 °C
4350 psi
@Strain 1 %,
Temperature 73.4 °F
ISO 527
 40.0 MPa
@Strain 1 %,
Temperature -20.0 °C
5800 psi
@Strain 1 %,
Temperature -4.00 °F
ISO 527
 40.0 MPa
@Strain 3 %,
Temperature 60.0 °C
5800 psi
@Strain 3 %,
Temperature 140 °F
ISO 527
 80.0 MPa
@Strain 3 %,
Temperature 23.0 °C
11600 psi
@Strain 3 %,
Temperature 73.4 °F
ISO 527
 100 MPa
@Strain 3 %,
Temperature -20.0 °C
14500 psi
@Strain 3 %,
Temperature -4.00 °F
ISO 527
Tensile Strength, Yield 90.0 MPa13100 psi50mm/min; ISO 527
Elongation at Yield 4.0 %4.0 %50mm/min; ISO 527
Modulus of Elasticity 3.40 GPa493 ksiISO 527
Flexural Modulus 3.00 GPa435 ksiISO 178
Izod Impact, Notched (ISO) 5.00 kJ/m²2.38 ft-lb/in²ISO 180/A
 5.00 kJ/m²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
ISO 180/A
Charpy Impact Unnotched 25.0 J/cm²119 ft-lb/in²ISO 179/1eU
 20.0 J/cm²
@Temperature -30.0 °C
95.2 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.400 J/cm²1.90 ft-lb/in²ISO 179/1eA
 0.300 J/cm²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC 60093
Dielectric Constant 3.3
@Frequency 1e+6 Hz
3.3
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.030
@Frequency 1e+6 Hz
0.030
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VTest Solution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 70.0 - 100 µm/m-°C
@Temperature 23.0 - 80.0 °C
38.9 - 55.6 µin/in-°F
@Temperature 73.4 - 176 °F
ISO 11359-1/-2
Specific Heat Capacity 1.70 J/g-°C0.406 BTU/lb-°F
Thermal Conductivity 0.300 W/m-K2.08 BTU-in/hr-ft²-°FDIN 52612
Melting Point 220 °C428 °FDIN 53752
Maximum Service Temperature, Air 87.0 °C189 °Ffor 50% loss of tensile strength after 20,000 hr
 97.0 °C207 °Ffor 50% loss of tensile strength after 5,000 hr
 180 °C356 °FISO 11359-1/-2
Deflection Temperature at 0.46 MPa (66 psi) 180 °C356 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C149 °FISO 75
Flammability, UL94 V-2
@Thickness >=1.50 mm
V-2
@Thickness >=0.0590 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 - 270 °C482 - 518 °FInjection-molding/Extrusion
Mold Temperature 40.0 - 60.0 °C104 - 140 °FInjection-molding
 
Descriptive Properties
ColorNatural
Commercial StatusNorth America and Europe
Impact ModifiedNo
Primary Processing TechniqueInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultramid® B3S Q661 PA6 (Dry)
BASF Ultramid® B3S HP PA6 (Conditioned)
BASF Ultramid® B3S BK00464 PA6 (Dry)
BASF Ultramid® B3S BK00464 PA6 (Conditioned)
BASF Ultramid® B3L PA6 (Dry)

PBASF9327 / 85091

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.