MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

SABIC LNP™ THERMOCOMP™ Compound D251RC Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP THERMOCOMP D251RC compound is based on recycled Polycarbonate (PC) resin containing 20% glass fiber. Added features of this grade include: High Modulus, Low Warpage, Good Ductility, Non-Brominated & Non-Chlorinated Flame Retardant. Post-Consumer Recycling (PCR) Polycarbonate content up to 35%.

Features: Post-Consumer Recycled (PCR) content,High Stiffness,Enhanced Ductility,Flame Retardant,Non-Chlorinated,Non-Brominated,Low Warpage,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.35 g/cc0.0488 lb/in³ASTM D792
Water Absorption 0.030 %
@Time 86400 sec
0.030 %
@Time 24.0 hour
ISO 62-1
Moisture Absorption 0.0200 %0.0200 %Injection Molding
Viscosity  10 cP
@Load 1.20 kg,
Temperature 300 °C
10 cP
@Load 2.65 lb,
Temperature 572 °F
MVR cc/10 min; ISO 1133
 21 cP
@Load 2.16 kg,
Temperature 300 °C
21 cP
@Load 4.76 lb,
Temperature 572 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0020 - 0.0040 cm/cm0.0020 - 0.0040 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0020 - 0.0040 cm/cm0.0020 - 0.0040 in/in24hrs; ASTM D955
Melt Flow  12 g/10 min
@Load 1.20 kg,
Temperature 300 °C
12 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
 25 g/10 min
@Load 2.16 kg,
Temperature 300 °C
25 g/10 min
@Load 4.76 lb,
Temperature 572 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 107 MPa15500 psi5 mm/min; ISO 527
 109 MPa15800 psi5 mm/min; ASTM D638
Elongation at Break 2.6 %2.6 %5 mm/min; ASTM D638
 2.6 %2.6 %5 mm/min; ISO 527
Tensile Modulus 6.65 GPa965 ksi1 mm/min; ISO 527
 6.70 GPa972 ksi5 mm/min; ASTM D638
Flexural Strength 158 MPa22900 psibrk, 1.3 mm/min, 50 mm span; ASTM D790
 160 MPa23200 psibreak, 2mm/min; ISO 178
 161 MPa23400 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
 161 MPa23400 psiyield, 2 mm/min; ISO 178
Flexural Modulus 6.05 GPa877 ksi1.3 mm/min, 50 mm span; ASTM D790
 6.15 GPa892 ksi2 mm/min; ISO 178
Izod Impact Notched 140 J103 ft-lbASTM D256
 90.0 J
@Temperature -30.0 °C
66.4 ft-lb
@Temperature -22.0 °F
ASTM D256
Izod Impact, Unnotched 6.80 J/cm12.7 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 13.0 kJ/m²6.19 ft-lb/in²80*10*4; ISO 180/1A
 9.00 kJ/m²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 41.0 kJ/m²19.5 ft-lb/in²80*10*4; ISO 180/1U
Dart Drop, Total Energy 22.0 J16.2 ft-lbASTM D3763
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cmASTM D257
Surface Resistance >= 1.00e+16 ohm>= 1.00e+16 ohmASTM D257
Dielectric Constant  3.25
@Frequency 1.10e+9 Hz
3.25
@Frequency 1.10e+9 Hz
SABIC method
 3.26
@Frequency 1.90e+9 Hz
3.26
@Frequency 1.90e+9 Hz
SABIC method
 3.26
@Frequency 5.00e+9 Hz
3.26
@Frequency 5.00e+9 Hz
SABIC method
 3.26
@Frequency 1e+10 Hz
3.26
@Frequency 1e+10 Hz
SABIC method
Dissipation Factor  0.0068
@Frequency 1.10e+9 Hz
0.0068
@Frequency 1.10e+9 Hz
SABIC method
 0.0069
@Frequency 1.90e+9 Hz
0.0069
@Frequency 1.90e+9 Hz
SABIC method
 0.0071
@Frequency 5.00e+9 Hz
0.0071
@Frequency 5.00e+9 Hz
SABIC method
 0.0073
@Frequency 1e+10 Hz
0.0073
@Frequency 1e+10 Hz
SABIC method
Comparative Tracking Index 175 - 250 V175 - 250 VUL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  25.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
13.9 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 26.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
14.4 µin/in-°F
@Temperature 73.4 - 176 °F
ASTM E831
CTE, linear, Transverse to Flow  63.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
35.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 75.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
41.7 µin/in-°F
@Temperature 73.4 - 176 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 121 °C250 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 120 °C
@Thickness 3.20 mm
248 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 116 °C241 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 115 °C
@Thickness 3.20 mm
239 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 122 °C252 °FRate B/50; ISO 306
 125 °C257 °FRate B/120; ISO 306
UL RTI, Electrical 80.0 °C176 °FUL 746B
UL RTI, Mechanical with Impact 80.0 °C176 °FUL 746B
UL RTI, Mechanical without Impact 80.0 °C176 °FUL 746B
Flammability, UL94  V-1
@Thickness >=0.500 mm
V-1
@Thickness >=0.0197 in
UL 94
 V-0
@Thickness >=0.600 mm
V-0
@Thickness >=0.0236 in
UL 94
Glow Wire Ignition Temperature  850 °C
@Thickness 1.00 mm
1560 °F
@Thickness 0.0394 in
IEC 60695-2-13
 850 °C
@Thickness 1.60 mm
1560 °F
@Thickness 0.0630 in
IEC 60695-2-13
 850 °C
@Thickness 2.00 mm
1560 °F
@Thickness 0.0787 in
IEC 60695-2-13
Glow Wire Flammability Index  960 °C
@Thickness 1.00 mm
1760 °F
@Thickness 0.0394 in
IEC 60695-2-12
 960 °C
@Thickness 1.60 mm
1760 °F
@Thickness 0.0630 in
IEC 60695-2-12
 960 °C
@Thickness 2.00 mm
1760 °F
@Thickness 0.0787 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 285 - 305 °C545 - 581 °F
Zone 2 270 - 290 °C518 - 554 °F
Zone 3 280 - 300 °C536 - 572 °F
Melt Temperature 285 - 310 °C545 - 590 °FInjection Molding
Mold Temperature 80.0 - 110 °C176 - 230 °F
Drying Temperature 110 °C230 °FInjection Molding
Dry Time 3.00 - 6.00 hour3.00 - 6.00 hourInjection Molding
Back Pressure 0.100 - 0.300 MPa14.5 - 43.5 psi
Screw Speed 50 - 90 rpm50 - 90 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81482 / 289429

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.