MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

A. Schulman Alcryn® 2265 UT Melt Processable Rubber
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Elastomer, Melt-Processible Rubber

Material Notes: Alcryn melt-processable rubber (MPR) is a true rubber, based on a partially cross-linked, chlorinated olefin interpolymer alloy. Alcryn is designed for the manufacture of rubber parts with high productivity on thermoplastic processing equipment.

Applications:

  • Window and door weatherstripping (and other complex profile extrusions)
  • Soft handles and grips
  • Molded seals and gaskets
  • Injection-molded and co-injection molded parts
  • Blow-molded parts
  • Tubing and hose
  • Wire and cable jackets
  • Coated fabrics and sheet goods
  • Information provided by Advanced Polymer Alloys

    Former product line of Advanced Polymer Alloys (APA), acquired by A. Schulman in 2014.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Specific Gravity 1.08 g/cc1.08 g/ccASTM D471; ISO 2781
    Viscosity 390000 cP
    @Shear Rate 300 1/s,
    Temperature 190 °C
    390000 cP
    @Shear Rate 300 1/s,
    Temperature 374 °F
    ASTM D3835
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Shore A 6262ASTM D2240; ISO 48
     6666After 7 days at 257°F (125°C); ASTM D573; ISO 188
    Tensile Strength, Ultimate 9.72 MPa1410 psiASTM D412; ISO 37
     11.5 MPa1670 psiAfter 7 days at 257°F (125°C); ASTM D573; ISO 188
    Elongation at Break 405 %405 %After 7 days at 257°F (125°C); ASTM D573; ISO 188
     470 %470 %ASTM D412; ISO 37
    100% Modulus  3.59 MPa
    @Strain 100 %
    520 psi
    @Strain 100 %
    ASTM D412; ISO 37
     4.41 MPa
    @Strain 100 %
    640 psi
    @Strain 100 %
    After 7 days at 257°F (125°C); ASTM D573; ISO 188
    Graves Tear Strength 26.3 kN/m
    @Temperature 23.9 °C
    150 pli
    @Temperature 75.0 °F
    Die C; ASTM D624
    Taber Abrasion, mg/1000 Cycles 7.07.0Cs-17 Wheel, 1000 g Load; ASTM D3389
    Compression Set 54 %
    @Temperature 100 °C
    54 %
    @Temperature 212 °F
    22 hrs.; ASTM D395; ISO 815
     12 %
    @Temperature 24.0 °C,
    Time 79200 sec
    12 %
    @Temperature 75.2 °F,
    Time 22.0 hour
    ASTM D395; ISO 815
    Tensile Set 6.0 %6.0 %ASTM D412
    Torsional Stiffness 2.515 MPa364.7 psiAt 75°F (24°C); ASTM D1043
     5.512 MPa799.4 psiAt -4°F (-20°C); ASTM D1043
     
    Thermal PropertiesMetricEnglishComments
    Brittleness Temperature -91.1 °C-132 °FASTM D746; ISO 812
    Clash Berg Stiffness Temperature -50.0 °C-58.0 °FAt 10,000 psi (69 Mpa); ASTM D1043
     
    Processing PropertiesMetricEnglishComments
    Processing Temperature 166 °C330 °F
     
    Descriptive Properties
    Fluid Resistance - Volume Change, % (ASTM D471)19After 7 Days in ASTM Ref. Fuel No. B at 75°F (24°C)
     -21After 7 Days in ASTM Oil No.1 at 212°F (100°C)
     23After 7 Days in IRM 903 Oil No.3 at 212°F (100°C)
     6After 7 Days in Water at 212°F (100°C)

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    A. Schulman POLYAXIS® LPA815 LPA 815EVA
    ExxonMobil Santoprene® 101-64 Thermoplastic Elastomer
    Polymax® Maxelast® C4630 TPE, Transparent
    Teknor Apex TEKRON® 4000-25 Thermoplastic Elastomer
    Advanced Elastomer Systems Santoprene® 153-38 Thermoplastic Rubber

    PAPA016 / 24083

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.