MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Samyang Tribit® 1501N PBT, Flame Retardancy
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Flame Retardant

Material Notes: Crystallization is fast, formability is excellent and thermal resistance, chemical resistance, electrical properties and abrasion resistance are excellent.
1501N is a V-2 flame retardancy grade.

Applications: Connectors (insulation characteristics)

Information provided by Samyang.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.38 g/cc1.38 g/ccASTM D792
Water Absorption 0.080 %0.080 %ASTM D570
Linear Mold Shrinkage 0.0020 - 0.012 cm/cm0.0020 - 0.012 in/inASTM D955
Melt Flow 60 g/10 min
@Load 2.16 kg,
Temperature 235 °C
60 g/10 min
@Load 4.76 lb,
Temperature 455 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 118118ASTM D785
Tensile Strength 53.9 MPa7820 psiASTM D638
Elongation at Break 40 %40 %ASTM D638
Flexural Yield Strength 80.4 MPa11700 psiASTM D790
Flexural Modulus 2.26 GPa327 ksiASTM D790
Izod Impact, Notched 0.588 J/cm
@Thickness 3.17 mm
1.10 ft-lb/in
@Thickness 0.125 in
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmASTM D257
Dielectric Constant 3.23.2ASTM D150
Dielectric Strength 18.0 kV/mm457 kV/inASTM D149
Dissipation Factor 0.0200.020ASTM D150
Arc Resistance 71 sec71 secASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear 90.0 µm/m-°C50.0 µin/in-°FASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 150 °C302 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C140 °FASTM D648
Flammability, UL94 V-2
@Thickness 0.810 mm
V-2
@Thickness 0.0319 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Samyang Tribit® 1700S Polybutylene Terephthalate
Samyang Tribit® 1503S Polybutylene Terephthalate
Samyang Tribit® 1500N Polybutylene Terephthalate, Flame Retardant
Samyang Tribit® 1500 Polybutylene Terephthalate

PSANX938 / 133332

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.