MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Asahi Kasei Leona™ FH772 Polyamide 66, GF Reinforced, Flame Retardant
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Glass Fiber Filled, Flame Retardant

Material Notes: Applications: Automotive parts, electrical & electronic parts, parts for office furnishings.

Information provided by Asahi Kasei Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.41 g/ccDry as Molded; ASTM D792
Density 1.41 g/ccDry as Molded; ISO 1183
Moisture Absorption at Equilibrium 1.3 %
@Temperature 23.0 °C
50% RH; ISO 62
 1.3 %
@Temperature 23.0 °C
50% RH
Linear Mold Shrinkage, Flow 0.0040 - 0.012 cm/cmAsahi Kasei
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 94.0 MPaDry as Molded; ISO 527
 136 MPaConditioned at 50% RH; ISO 527
Tensile Strength 150 MPaDry as Molded; ASTM D638
Elongation at Break 3.0 %Dry as Molded; ISO 527
 5.0 %Conditioned at 50% RH; ISO 527
Tensile Modulus 6700 MPaConditioned at 50% RH; ISO 527
 9800 MPaDry as Molded; ISO 527
Flexural Strength 154 MPaConditioned at 50% RH; ISO 178
 209 MPaDry as Molded; ISO 178
Flexural Modulus 6600 MPaConditioned at 50% RH; ISO 178
 9600 MPaDry as Molded; ISO 178
Izod Impact, Notched 75.0 J/mDry as Molded; ASTM D256
Charpy Impact Unnotched 58.0 kJ/m²Conditioned at 50% RH; ISO 179
 58.0 kJ/m²Dry as Molded; ISO 179
Charpy Impact, Notched 8.00 kJ/m²Dry as Molded; ISO 179
 10.0 kJ/m²Conditioned at 50% RH; ISO 179
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 600 V
@Thickness 3.00 mm
Dry as Molded; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 30.0 µm/m-°CDry as Molded; ASTMD 696
Deflection Temperature at 0.46 MPa (66 psi) 258 °CDry as Molded; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 241 °CDry as Molded; ISO 75
Flammability, UL94 V-0
@Thickness 0.750 mm
Dry as Molded
Glow Wire Flammability Index 960 °CDry as Molded; IEC 60695-2-12

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Nylon 66, 20% Glass Fiber Filled
Eurotec® Tecomid® NA40 GR25 NL XA60 PA6.6, 25% glass fiber reinforced, flame retardant - halogen & red phosphorus free, heat stabilized, natural
BASF Ultramid® A3UG5 BK 23260 25% Glass Filled PA66 (Dry)

PASAHI8167 / 221194

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.