MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
TIMET TIMETAL® 679 (Ti-11Sn-5Zr-2.25Al-1Mo-0.2Si) Titanium Alloy; Oil Quenched & Aged
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Beta Titanium Alloy

Material Notes: High-Temperature, High-Strength Creep Resistant Alloy

Industry Specifications: USA Aerospace: AMS 4974.

TIMETAL 679 has excellent tensile strength and is creep resistant up to 450°C. It is a three-phase alloy at room temperature, having an alpha + beta + compound field and a maximum processing temperature of 925°C is recommended. It is nonmagnetic.

Typical heat treatment for this alloy: Solution heat treatment: 900°C for 30 min. Aging heat treatment: 500°C for 24 hrs, air cool.

Data provided by TIMET.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 4.84 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 899 MPa
@Temperature 450 °C
 932 MPa
@Temperature 400 °C
 986 MPa
@Temperature 300 °C
 1021 MPa
@Temperature 200 °C
 >= 1110 MPa
@Temperature 20.0 °C
 1118 MPa
@Temperature 100 °C
Tensile Strength, Yield 688 MPa
@Strain 0.2 %,
Temperature 450 °C
 701 MPa
@Strain 0.2 %,
Temperature 400 °C
 738 MPa
@Strain 0.2 %,
Temperature 300 °C
 819 MPa
@Strain 0.2 %,
Temperature 200 °C
 940 MPa
@Strain 0.2 %,
Temperature 100 °C
 >= 970 MPa
@Strain 0.2 %,
Temperature 20.0 °C
Elongation at Break >= 8.0 %
@Temperature 20.0 °C
in 5D
 14 %
@Temperature 100 °C
in 5D
 14 %
@Temperature 300 °C
in 5D
 14 %
@Temperature 400 °C
in 5D
 14 %
@Temperature 450 °C
in 5D
 15 %
@Temperature 200 °C
in 5D
Reduction of Area >= 25 %
@Temperature 20.0 °C
 43 %
@Temperature 100 °C
 45 %
@Temperature 450 °C
 46 %
@Temperature 200 °C
 46 %
@Temperature 300 °C
 46 %
@Temperature 400 °C
Modulus of Elasticity 107 GPaTypical
Notched Tensile Strength >= 1480 MPa
Shear Modulus 46.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000160 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 8.30 µm/m-°C
@Temperature 20.0 °C
Thermal Conductivity 8.30 W/m-K
Maximum Service Temperature, Air 450 °CCreep Resistance Maintained
Beta Transus 950 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 2.0 - 2.5 %
Hydrogen, H <= 0.0125 %
Iron, Fe <= 0.20 %
Molybdenum, Mo 0.80 - 1.2 %
Oxygen, O <= 0.20 %
Silicon, Si 0.10 - 0.50 %
Tin, Sn 10.5 - 11.5 %
Titanium, Ti 77.9 - 82.6 %Calculated as remainder
Zirconium, Zr 4.0 - 6.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
TIMET TIMETAL® 6-4 ELI Titanium Alloy (Ti-6Al-4V ELI; ASTM Grade 23) (Solution Treated; 0.025 - 1.000 in Sheet and Plate; Per ASTM B265)
TIMET 6-6-2 Titanium Alloy (Ti-6Al-6V-2Sn), Solution Treated and Aged
TIMET TIMETAL® 6-2-4-6 Titanium Alloy (Ti-6Al-2Sn-4Zr-6Mo), 50% Equiaxed Alpha + STOA
TIMET TIMETAL® 6-2-4-6 Titanium Alloy (Ti-6Al-2Sn-4Zr-6Mo), Beta Forged + STA
ATI Allvac® Vasco® Greek Ascoloy Specialty Steel, Heat Treatment: 871°C (1600°F) + Age

NTIME679 / 19336

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.