MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Latrobe Nitralloy® N™ VAC-ARC Premium Nitriding Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Carbon Steel; High Carbon Steel

Material Notes: NITRALLOY N is an age hardenable nitriding steel. The age hardening capability of the alloy permits the core strength to be developed while the surface is being nitrided. VAC-ARC remelting is employed to provide preferred ingot solidification and superior microcleanliness.

Tensile properties are that of the core.

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 29Core, At 1650°F, oil quench, tempered at 1200°F
 41Core, A+ age at 975°C for 20 hours
Tensile Strength, Ultimate 132 ksiAt 1650°F, oil quench, tempered at 1200°F
 180 ksiA+ age at 975°C for 20 hours
Tensile Strength, Yield 1172 MPaA+ age at 975°C for 20 hours
 793 MPa
@Temperature 899 °C
oil quench, tempered at 1200°F
Elongation at Break 16 %A+ age at 975°C for 20 hours
 22 %
@Temperature 899 °C
sample was oil quenched and tempered at 1200°F
Reduction of Area 50 %A+ age at 975°C for 20 hours
 59 %
@Temperature 899 °C
after oil quench, tempered at 1200°F
Charpy Impact 16.3 J48 Aging at 504°C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 1.25 %
Carbon, C 0.24 %
Chromium, Cr 1.15 %
Iron, Fe 92.71 %
Manganese, Mn 0.60 %
Molybdenum, Mo 0.25 %
Nickel, Ni 3.5 %
Silicon, Si 0.30 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Latrobe Nitralloy® 135 Modified VAC-ARC, Up to 1.5 in Premium Nitriding Steel
Latrobe Nitralloy® 135 Modified VAC-ARC, 3 to 5 in Premium Nitriding Steel
Latrobe Nitralloy® 135 Modified VAC-ARC, 1.5 to 3 in Premium Nitriding Steel
AISI 5120 Steel, heat treated, machined to 13.7 mm, pseudocarburized, 150°C (300°F) temper
Carpenter AerMet® 310

NTIMK009 / 19357

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.