MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

Celanese CoolPoly® E5105 Thermally Conductive Polyphenylene Sulfide
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS)

Material Notes: CoolPoly E series of thermally conductive plastics transfers heat, a characteristic previously unavailable in injection molding grade polymers. CoolPoly is lightweight, netshape moldable and allows design freedom in applications previously restricted to metals. The E series is electrically conductive and provides inherent EMI/RFI shielding characteristics.

CoolPoly E5105 is a thermally conductive injection molding resin based on a polyphenylene sulfide (PPS) matrix. CoolPoly E5105 is electrically conductive. Thermally conductive polymers like CoolPoly E5105 cool faster than standard injection molding grade resins.

Information provided by Cool Polymers, Inc.

Celanese acquired Cool Polymers in 2014.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.49 g/cc0.0538 lb/in³ISO 1183
Water Absorption 0.10 %0.10 %ISO 62
Linear Mold Shrinkage 0.0050 - 0.0080 cm/cm0.0050 - 0.0080 in/inASTM D551
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 60.0 MPa8700 psiISO 527-1
Elongation at Break 0.80 %0.80 %ISO 527-1
Tensile Modulus 10.0 GPa1450 ksiISO 527-1
Flexural Strength 90.0 MPa13100 psiISO 178
Flexural Modulus 8.95 GPa1300 ksiISO 178
Charpy Impact Unnotched 0.930 J/cm²4.43 ft-lb/in²ISO 179-1
Charpy Impact, Notched 0.180 J/cm²0.857 ft-lb/in²ISO 179-1
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 1.15 J/g-°C0.275 BTU/lb-°FASTM E1461
Thermal Conductivity 4.50 W/m-K31.2 BTU-in/hr-ft²-°FASTM E1461
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 290 - 315 °C554 - 599 °F
Middle Barrel Temperature 300 - 320 °C572 - 608 °F
Front Barrel Temperature 310 - 330 °C590 - 626 °F
Nozzle Temperature 310 - 335 °C590 - 635 °F
Melt Temperature 307 - 332 °C585 - 630 °F
Mold Temperature 135 - 177 °C275 - 351 °F
Drying Temperature 150 °C302 °F
Dry Time 6 hour6 hour
Moisture Content 0.20 %0.20 %
Dew Point -40.0 °C-40.0 °F
Injection Pressure 62.0 - 165 MPa8990 - 23900 psi
Hold Pressure 40.0 - 105 MPa5800 - 15200 psi
Back Pressure 0.200 - 0.500 MPa29.0 - 72.5 psi
Screw Speed 40 - 80 rpm40 - 80 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese CoolPoly® D5108 Thermally Conductive Polyphenylene Sulfide
Celanese CoolPoly® E3603 Thermally Conductive Polyphthalamide (PPA)
Celanese Coolpoly® D1202 Thermally Conductive Polypropylene
Celanese CoolPoly® E5101 Thermally Conductive Polyphenylene Sulfide
Celanese CoolPoly® E1201 Thermally Conductive Polypropylene

PCOOL38 / 29027

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.