MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Nilit Nilamid A3 N H2 Nucleated, Heat Stabilized Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Heat Stabilized

Material Notes: Description: Nilamid A3 N H2 is a nucleated, heat stabilized NYLON 66 with excellent flow characteristics and very fast cycle time. It is widely used throughout many industries for mass production articles that require fast cycle times and good resistance against thermal aging, like for instance terminal blocks or automotive connectors.

Key characteristics:

  • Excellent flow
  • Fast cycle time
  • High elongation
  • Good mould release
  • High toughness
  • Good thermal performance
  • UL 94 V2 listed down to 0.75 mm

Information provided by NILIT.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³ASTM D792, ISO 1183
Water Absorption 1.2 %1.2 %23°C, 24h in H2O; sim. ISO 62
Water Absorption at Saturation 8.0 %8.0 %sim. ISO 62
Linear Mold Shrinkage, Flow 0.013 cm/cm0.013 in/inEuronil
Linear Mold Shrinkage, Transverse 0.013 cm/cm0.013 in/inEuronil
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 85.0 MPa12300 psiISO 527, ASTM D638
Elongation at Break >= 40 %>= 40 %ISO 527, ASTM D638
Elongation at Yield 4.0 %4.0 %ISO 527, ASTM D638
Tensile Modulus 3.00 GPa435 ksiISO 527, ASTM D638
Flexural Yield Strength 115 MPa16700 psiISO 178, ASTM D790
 35.0 MPa
@Temperature 90.0 °C
5080 psi
@Temperature 194 °F
ISO 178, ASTM D790
Flexural Modulus 3.20 GPa464 ksiISO 178, ASTM D790
 0.750 GPa
@Temperature 90.0 °C
109 ksi
@Temperature 194 °F
ISO 178, ASTM D790
Izod Impact, Notched (ISO)  3.50 kJ/m²
@Temperature -30.0 °C
1.67 ft-lb/in²
@Temperature -22.0 °F
ISO 180/1A
 4.50 kJ/m²
@Temperature 23.0 °C
2.14 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Charpy Impact Unnotched NBNBISO 179
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179
Charpy Impact, Notched 0.550 J/cm²2.62 ft-lb/in²ISO 179
 0.400 J/cm²
@Temperature -30.0 °C
1.90 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 18.0 kV/mm
@Thickness 2.00 mm
457 kV/in
@Thickness 0.0787 in
ASTM D149
Comparative Tracking Index  550 V
@Thickness 3.20 mm
550 V
@Thickness 0.126 in
Sol. B; IEC 112, UL 746A
 600 V
@Thickness 3.20 mm
600 V
@Thickness 0.126 in
Sol. A; IEC 112, UL 746A
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 115 °C239 °F20,000 hr; IEC 216
Deflection Temperature at 0.46 MPa (66 psi) 235 °C455 °FISO 75, ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 93.0 °C199 °FISO 75, ASTM D648
Vicat Softening Point 245 °C473 °F49 N; ISO 306, ASTM D1525
 255 °C491 °F9.8 N; ISO 306, ASTM D1525
Flammability, UL94  V-2
@Thickness 1.60 mm
V-2
@Thickness 0.0630 in
 V-2
@Thickness 0.400 mm
V-2
@Thickness 0.0157 in
 V-2
@Thickness 0.800 mm
V-2
@Thickness 0.0315 in
 V-2
@Thickness 3.20 mm
V-2
@Thickness 0.126 in
Oxygen Index 26 %26 %ASTM D2863
Glow Wire Flammability Index  850 °C
@Thickness 0.800 mm
1560 °F
@Thickness 0.0315 in
IEC 694-2-12
 850 °C
@Thickness 3.20 mm
1560 °F
@Thickness 0.126 in
IEC 694-2-12
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 265 - 295 °C509 - 563 °F
Zone 1 260 - 290 °C500 - 554 °Fhopper
Zone 2 265 - 290 °C509 - 554 °F
Zone 3 265 - 290 °C509 - 554 °F
Zone 4 265 - 295 °C509 - 563 °F
Melt Temperature 270 - 290 °C518 - 554 °FDo not melt above 300°C
Mold Temperature 60.0 - 80.0 °C140 - 176 °F80°C is Preferred
Drying Temperature 80.0 - 85.0 °C176 - 185 °F
Dry Time 4 hour4 hour
Injection Pressure 70.0 - 100 MPa10200 - 14500 psi
 
Descriptive Properties
Clamping Forcein tons, 0.7 times the projected surface area in cm2
Flammability RatingSEFMVSS No. 302, 355x100x1 mm
Heat Resistance - Ball TestOKat 125°C, IEC 309
 OKat 165°C, IEC 309
Holding Pressure90 Mpa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Nilit Nilamid A3 H6 G6 30% Glass Reinforced PA66
Celanese Nilit Nilamid A3 H ZC High Impact PA66
Domo Technyl® A218 Heat Stabilized Nylon 66
Celanese Zytel® MT409AHS BK010 PA66-I
Celanese Nilit Nilamid B3N Unfilled, Nucleated PA6

PLBN21 / 50410

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.